Tool Steel Machinability Rating Chart (W1 = 100 Basis) | Aobo Steel
Tool Steel Machining Data

Tool Steel Machinability Rating Chart

Approximate machinability ratings for annealed tool steels, on the scale where the water-hardening grades W1, W2 and W5 = 100. Ratings cover the full AISI tool steel range, from O6 (125) to the high-vanadium grades (25-30).

100 = W1, W2, W5 (basis) 125 easier to machine than W 30-40 range across grades (a)(b) footnote
Tool steel typesMachinability rating
O6125
W1, W2, W5100 (a)
A1090
P2, P3, P4, P5, P675-90
P20, P2165-80
L2, L665-75
S1, S2, S5, S6, S760-70
H10, H11, H13, H14, H1960-70 (b)
O1, O2, O745-60
A2, A3, A4, A6, A8, A945-60
H21, H22, H24, H25, H26, H4245-55 (b)
T140-50
M240-50
T435-40
M3, clase 135-40
D2, D3, D4, D5, D7, A730-40
T1525-30
M1525-30
  • (a) Equivalent to approximately 30% of the machinability of B1112 free-machining constructional steel.
  • (b) For hardness range 150 to 200 HB.

Notas de la tabla

Ratings are relative to the water-hardening tool steels (W1, W2, W5 = 100) in the annealed condition — a higher number means easier machining. Because the tool-steel scale differs from the constructional-steel scale, 100 here is only about 30% of B1112 (=100 on the constructional scale).

Annealing condition and hardness strongly affect machinability; grades marked (b) are rated for the 150-200 HB range. Improve machinability by specifying the annealed condition or a resulfurized variant where the grade allows it.

Reference data for comparison — confirm the delivered condition and hardness with your supplier before planning machining times.

Source: ASM Handbook, Volume 1 — Properties and Selection: Irons, Steels, and High-Performance Alloys, Table 15 “Approximate machinability ratings for annealed tool steels” (10th ed.). Reference data for comparison — verify the delivered condition before planning machining.