Tool Steel Tempering Chart

Tempering temperatures, the hardness each one produces, and the oxide colors used to judge temperature on the shop floor. Covers D2, D3, D4, D5, D7, O1, O2, O6, O7, A2, A6, A7, A8, H10 to H23, M2, M4 and M42, with metric and imperial values.

Tempering temperature and working hardness

Six grades cover most die and tool work, with the hardness at which each is normally put into service. Quench temperatures and the full quench-and-temper schedule are in the hardening and tempering chart.

GradeTypeAs-quenched HRC (a)Working HRCRecommended tempering, °F°C
A2Cold work, air-hardening6458–60400–450204–232
D2Cold work, high-chromium6458–60900–960482–516
H13Hot work, chromium5440–481050–1150566–621
M2High-speed molybdenum6562–641000–1050538–566
O1Cold work, oil-hardening6458–60400–450204–232
S7Shock-resisting6056–58400–450204–232

Source: Tool and Die Making Troubleshooter (R. M. Leed), Table 8-7, from Bethlehem Steel data.

Tool Steel Tempering Chart, printable PDF

Three A4 pages with the tempering windows for 28 grades, the H13 and M2 hardness data, the oxide tempering colors, and our contact details.

Tempering windows by grade

Hardening and tempering data for the tool steels most often quoted and stocked. Grouped by family, with the approximate hardness span across the window. Each grade’s chemistry is in the tool steel composition chart.

GradeTypeTempering temperature, °F°CApprox. tempered hardness, HRC (c)
High-speed tool steels
M2Molybdenum high speed1000–1160538–62765–60
M4Molybdenum high speed, vanadium1000–1100538–59366–61
M7Molybdenum high speed1000–1100538–59366–61
M10Molybdenum high speed1000–1100538–59365–60
M42Cobalt high speed950–1100510–59370–65
Hot-work tool steels
H10Chromium hot work1000–1200538–64956–39
H11Chromium hot work1000–1200538–64954–38
H12Chromium-tungsten hot work1000–1200538–64955–38
H13Chromium hot work1000–1200538–64953–38
H19Chromium-cobalt hot work1000–1300538–70459–40
H21Tungsten hot work1100–1250593–67754–36
H23Tungsten hot work1200–1500649–81647–30
Cold-work tool steels
D2High-chromium cold work400–1000204–53861–54
D3High-chromium cold work400–1000204–53861–54
D4High-chromium cold work400–1000204–53861–54
D5High-chromium cold work400–1000204–53861–54
D7High-chromium cold work300–1000149–53865–58
A2Medium-alloy air-hardening350–1000177–53862–57
A6Medium-alloy air-hardening300–800149–42760–54
A7Medium-alloy air-hardening300–1000149–53867–57
A8Medium-alloy air-hardening350–1100177–59360–50
O1Oil-hardening cold work350–500177–26062–57
O2Oil-hardening cold work350–500177–26062–57
O6Oil-hardening cold work350–600177–31663–58
O7Oil-hardening cold work350–550177–28864–58
Shock-resisting tool steels
S1Shock-resisting400–1200204–64958–40
S5Shock-resisting350–800177–42760–50
S7Shock-resisting400–1150204–62157–45

Source: Machinery’s Handbook, 28th ed., tool steel tables 6, 8, 9 and 10 (high-speed, hot-work, cold-work and shock-resisting groups).

H13 at each tempering temperature

Hardness, tensile properties, and impact energy of H13 after double tempering. Same austenitizing temperature, two different quench routes. Hardness at the working temperature is in the hot hardness chart.

Tempering
°C
°FHardness
HRC
Tensile
MPa (ksi)
Yield
MPa (ksi)
Elongation
%
Charpy V-notch
at 21 °C, J (ft·lbf)
Oil quenched from 1010 °C (1850 °F), double tempered 2 + 2 h
527980521960 (284)1570 (228)13.016 (12)
5551030501835 (266)1530 (222)13.124 (18)
5751065481730 (251)1470 (213)13.527 (20)
5931100461580 (229)1365 (198)14.428.5 (21)
Air cooled from 1010 °C (1850 °F), double tempered 2 + 2 h
52497554———14 (10)
565105052———14 (10)
607112547———24 (18)

Source: ASM Handbook, Volume 1 (10th ed.), Ultrahigh-Strength Steels, Tables 31 and 33 (H13 round bar). The air-cooled series reports only hardness and impact energy.

M2 hardness against tempering temperature

The dip and recovery between 700 and 1050 °F is secondary hardening, which is why high-speed steel is tempered hot instead of just hard.

Tempering
°F
°CHardness after oil quench, HRCHardness after air quench, HRC
3001506666.5
4002056565
5002606463.5
6003156362.5
70037062.562.5
8004256362.5
9004806563.5
10005406663.5
10505656663.5
110059564.561.5
11506206260
120065053.553

Source: Heat Treatment, Selection and Application of Tool Steels (W. E. Bryson, 2nd ed.), Table 10.1, austenitized at 2250 °F (1230 °C).

Tempering colors

Oxide colors on plain carbon steel, used as a shop-floor cross-check when a pyrometer is not at hand.

°F°CColor of steel
430221Very pale yellow
440227Light yellow
450232Pale straw-yellow
460238Straw-yellow
470243Deep straw-yellow
480249Dark yellow
490254Yellow-brown
500260Brown-yellow
510266Spotted red-brown
520271Brown-purple
530277Light purple
540282Full purple
550288Dark purple
560293Full blue
570299Dark blue
640338Light blue

Source: Machinery’s Handbook, 28th ed., Table 1, temperatures indicated by the color of plain carbon steel. Other shop references list the same colors over slightly different ranges, for example, straw at 460 °F (238 °C) and blue at 580 °F (304 °C).

Tool Steel Tempering Chart, printable PDF

Three A4 pages with tempering windows for 28 grades, H13 and M2 hardness data, oxide tempering colors, and our contact details.

  • (a) As-quenched hardness, measured before tempering.
  • (b) Temperatures are printed here as published in each source. Celsius values in the tempered-hardness tables are converted from Fahrenheit and rounded to the nearest degree.
  • (c) Approximate tempered hardness is the span from the low end of the tempering window to the high end. The exact value depends on austenitizing temperature, quench, section size, and the number of tempers.

Table notes

Different references publish different tempering windows for the same grade because the outcome depends on how the part was austenitized, how fast it cooled, how thick it is and how many tempers it receives. D2, for example, is tempered at 900 to 960 °F (482 to 516 °C) to hold 58 to 60 HRC in shop practice, while Machinery’s Handbook lists a wider 400 to 1000 °F window with an approximate hardness span of 61 to 54 HRC. Treat both tables as starting windows, then confirm on your own furnace with a test piece.

  • Temper straight after quenching. Air-hardening and oil-hardening grades should reach the tempering furnace while the part is still warm, about 125 to 150 °F (50 to 65 °C). A quenched tool left at room temperature before the first temper carries a higher risk of cracking, and the delay costs nothing to avoid. Hold at temperature for one hour per inch of section, and use two hours per inch on large or complex sections. The defects that appear when a stage of the cycle is skipped, and the checks that correct them, are listed in the heat treatment troubleshooting chart.
  • Temper twice, and three times on high-speed steel. Air-hardening cold-work grades and molybdenum high-speed grades are normally tempered twice to convert retained austenite and stabilize the dimensions. Add a third temper for parts with a lot of detail or for hard-service tooling.
  • Never heat a tempered part above its tempering temperature. Stress relieving, straightening, or weld repair above that temperature softens the tool, so the tempering temperature sets a ceiling for every later operation.
  • Tempering colors are an indication only. The oxide colors in the last table were measured on plain carbon steel. Alloy content shifts them, so use a thermocouple or pyrometer for control and the colors as a cross-check on the shop floor.

The part should be at 125 to 150 °F (50 to 65 °C) when it enters the tempering furnace. Waiting until it is cold adds cracking risk on air-hardening grades.

Hold at temperature for one hour per inch of section, two hours per inch on heavy or complex blocks. Short soak times leave retained austenite and unstable dimensions.

Every point of hardness above the working range removes toughness. Some tempering bands lower toughness for a different reason, and the temperatures that trigger each one are listed on the steel embrittlement types page. Choose the range the die needs and stay within it rather than hardening to the steel’s maximum.

Tempering windows are grade- and mill-specific. Aobo Steel supplies heat treatment guidance with each order, and the mill certificate travels with the steel.

Tool steel annealing and normalizing temperatures · D2 austenitizing temperature · Tool steel forging temperature guide · Tool steel machinability ratings · H13 die casting applications · D2 tool steel machining guide

Sources: Machinery’s Handbook, 28th ed. (Industrial Press), tool steel tables 6, 8, 9 and 10 and Table 1 on temper colors; ASM Handbook, Volume 1 (10th ed.), Ultrahigh-Strength Steels, Tables 31 and 33; Tool and Die Making Troubleshooter (R. M. Leed), Tables 8-3 and 8-7; Heat Treatment, Selection and Application of Tool Steels (W. E. Bryson, 2nd ed.), Table 10.1. Reference data for comparison only. Confirm tempering practice with your heat treater and the mill data sheet before production.