Bulk tool steel bar stock in the Aobo Steel warehouse

Cr12Mo1V1 (D2 / 1.2379 / SKD11) Tool Steel Supplier from China

Standard D2 Grade | Bulk Supply for Distributors & Stockists

Cr12Mo1V1 steel is a high-carbon, high-chromium ledeburitic cold-work mold steel widely adopted internationally. It is also known by the American AISI/ASTM designation D2, the Japanese JIS designation SKD10 or SKD11, the German DIN designation X153CrMoV12-1 or 1.2379, and the Austrian Bohler designation K110.

Cr12Mo1V1 Tool Steel Supply Overview

GradeGB Cr12Mo1V1 / AISI D2 / DIN 1.2379 / JIS SKD11
Delivery ConditionFully Annealed (Soft Condition for Machining)
Available FormsRound Bar / Flat Bar / Plate / Forged Block
Monthly Production CapacityApprox. 1000 metric tons
Recommended Export QuantityFull 20GP container (~26 tons)
MOQ5 tons
Lead Time (With Ingot Stock)Approx. 20 days
Lead Time (Fresh Melt)30–45 days
Lead Time (ESR Grade)Approx. 60 days
InspectionIn-house UT team + Third-party inspection available
DocumentationMTC (EN 10204 3.1) + UT Report

Why Global Distributors Source Cr12Mo1V1 from Aobo Steel

  • Continuous monthly supply of around 1000 tons
  • MOQ from 5 tons for wholesale orders
  • Container-optimized bar and plate lengths
  • Mixed sizes are supported for export loading
  • Annealed delivery for downstream machining
  • Stable sourcing through integrated supply chain partners
  • UT inspection available to SEP 1921-82 D/d or E/e
  • MTC and batch traceability with each shipment
  • Heat number tracking for order control
  • Black, turned, and polished surface options
  • Bulk export packing for sea shipment
  • Clear conversion path to the dedicated bulk supply page

Stable Production for Long-Term Bulk Supply

  • Continuous monthly output of around 1000 tons
  • Continuous production cycles for inventory replenishment
  • ESR (Electro-Slag Remelting) is available upon request
  • Stable alloy sourcing to reduce supply interruption risk
  • Full batch traceability linked to the original heat number

Available Cr12Mo1V1 Tool Steel Forms

Quality Control for Bulk Orders

Every batch of tool steel supplied by Aobo Steel is verified before shipment to ensure grade accuracy, internal soundness, and traceability for bulk orders.

  • Chemical composition verified by a spectrometer
  • Ultrasonic testing available (SEP 1921-82)
  • Delivered in spheroidized annealed condition
  • Mill Test Certificate (EN 10204 3.1) with heat number
  • Dimensional and surface inspection before shipment

Export Packaging and Container Loading

  • Professional seaworthy export packing
  • 20GP loading optimized up to ~26 tons
  • Mixed grades and mixed sizes supported
  • Anti-rust protection for long sea transit

For international shipments, full-container loading is strongly recommended to ensure cost efficiency and smoother customs processing.

Composition(GB / T 1299—2000)

CSiMnCrMoVPSOther
1.40 – 1.60≤0.60≤0.6011.0 – 13.00.70 – 1.200.50 – 1.10≤0.030≤0.030Co ≤1.00

Physical Properties of Cr12Mo1V1 Steel

Critical Point Temperature

Critical PointAc₁AcₑₘAr₁ArₑₘMs
Temperature (Approx. value) /°C810875695750190

Linear Expansion Coefficient

Temperature/°C20 ~ 10020 ~ 20020 ~ 30020 ~ 400
Linear Expansion Coefficient α /× 10⁻⁶°C⁻¹10.511.511.912.2

Other Physical Properties

Modulus of Elasticity E/MPaSpecific Heat Capacity cₚ/[J/(kg·K)]
207000461

Forging Process Specification of Cr12Mo1V1 Steel

ItemHeating Temperature/°CInitial Forging Temperature/°CFinal Forging Temperature/°CCooling Method
Steel Ingot1120 ~ 11601050 ~ 1090≥850High-temperature annealing
Steel Billet1120 ~ 11401050 ~ 1070≥850High-temperature annealing, pit cooling, or sand cooling

Heat Treatment of Cr12Mo1V1 Steel

Preheating

PlanProcess Parameters
Forging blank, steel ingot annealing processHeating temperature is 840 ~ 860°C, hold for 2h; furnace cool to 720 ~ 740°C, hold for 4h, furnace cool to below 550°C, then air cool. Annealed hardness is 205-255 HBW.
Steel material isothermal annealing processHeating temperature is 840 ~ 860°C, hold for 2h; furnace cool to 720 ~ 740°C, hold for 4h, furnace cool to below 550°C, then air cool. Annealed hardness is 205 ~ 255 HBW.

Quenching

Heating Temperature/°CCoolingHardness HRC
Plan1st Preheat2nd PreheatQuench Heating
Ⅰ500 ~ 600820 ~ 860980 ~ 1040
Ⅱ500 ~ 600820 ~ 8601060 ~ 1100

Relationship between Quenching Temperature, Hardness, and Retained Austenite Content

Quenching Temperature/°C900950980100010301050108011001130
Hardness HRC52.557.56063.5646362.56260
Retained Austenite Content (Volume fraction, %)—444.56101324—

Tempering

Quenching PlanTempering Temperature/°CNumber of Tempering CyclesHardness HRC
Ⅰ180 ~ 230160 ~ 64
Ⅱ510 ~ 540260 ~ 64

The effect of tempering temperature on hardness

Quenching conditionTempering TemperatureUntempered (HRC)200°C250°C300°C350°C400°C450°C500°C550°C600°C650°C700°C
1010℃/air cooledHarndness(HRC)6260.559.558.55858585856484236.5
1010℃/oil quenchedHarndness(HRC)62.561.56058.558.558.558.559.556484236.5
1066℃/air cooledHarndness(HRC)6361.560.56059.559.559.560.561.5514340.5
1066℃/oil quenchedHarndness(HRC)6361.56059.559.559.5606162.5514438
1121℃/air cooledHarndness(HRC)60.559.55857.557575759.56251.54440.5
1121℃/oil quenchedHarndness(HRC)605858.5565454.556.55861574438

Cr12Mo1V1 Steel Impact Toughness vs. Tempering Temperature

Cr12Mo1V1 Steel Impact Toughness vs. Tempering Temperature

Effect of Tempering Temperature on the Torsional Impact Energy of Cr12Mo1V1 Steel

Effect of Tempering Temperature on the Torsional Impact Energy of Cr12Mo1V1 Steel

Mechanical Properties of Cr12Mo1V1 Steel

Cr12Mo1V1 steel is a high-carbon, high-chromium steel with high hardenability and wear resistance. Due to the higher content of Molybdenum (Mo) and Vanadium (V) elements compared to Cr12MoV steel, the as-cast structure within the steel is improved, the crystal grains are refined, and the carbide morphology is enhanced. Consequently, the steel exhibits superior mechanical properties, including tensile strength, hardness, and impact toughness, along with good wear resistance and higher tempering resistance. A comparison of the mechanical properties between Cr12Mo1V1 steel and Cr12MoV steel is shown in the Table.

Comparison of Mechanical Properties between Cr12Mo1V1 and Cr12MoV Steel

Quenching Temperature/°CSteel GradeBending Strength (σb)/MPaImpact Toughness (aK)/J/cm²Hardness HRC
1020Cr12Mo1V132624059.3
Cr12MoV28884061.0
1060Cr12Mo1V1155035.561.0
Cr12MoV7961061.5

Applications

Cr12Mo1V1 steel is primarily used to manufacture various high-precision, long-life cold-work molds, tools, and measuring instruments. Specific applications include:

  • Complex-shaped punching dies/cavity dies.
  • Silicon steel sheet blanking dies.
  • Trimming dies, rolling dies.
  • Wire drawing dies.
  • Cold extrusion dies.
  • Steel plate deep drawing dies.
  • Thread rolling dies/plates.
  • Cold shearing blades/circular saws.
  • Standard tools and gauges.
  • Plastic molds require high precision, long life, and wear resistance.
  • Used for heavy-duty, high-impact cold working applications.

Equivalent Grades

  • USA (ASTM/UNS): D2 / T30402
  • Japan (JIS): SKD11
  • Germany (DIN): 1.2379 / X155CrVMo12-1