Stainless Steel Physical Properties Chart

Density, elastic modulus, thermal expansion, thermal conductivity, specific heat, electrical resistivity and melting range for 48 wrought stainless steels in the annealed condition — austenitic, ferritic, martensitic (410, 420, 440A, 440C) and precipitation-hardening types. Metric values with imperial equivalents.

TypeUNS
number
Density
g/cm³
Elastic
modulus
GPa
Mean CTE from 0 °C (32 °F) toThermal conductivitySpecific
heat (a)
J/kg·K
Electrical
resistivity
nΩ·m
Magnetic
permeability (b)
Melting range
°C (°F)
100 °C315 °C538 °Cat 100 °Cat 500 °C
201S201007.8 (0.28)197 (28.6)15.7 (8.7)17.5 (9.7)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)6901.021400-1450 (2550-2650)
202S202007.8 (0.28)—17.5 (9.7)18.4 (10.2)19.2 (10.7)16.2 (9.4)21.6 (12.5)500 (0.12)6901.021400-1450 (2550-2650)
205S205007.8 (0.28)197 (28.6)—17.9 (9.9)19.1 (10.6)——500 (0.12)———
301S301008.0 (0.29)193 (28.0)17.0 (9.4)17.2 (9.6)18.2 (10.1)16.2 (9.4)21.5 (12.4)500 (0.12)7201.021400-1420 (2550-2590)
302S302008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)7201.021400-1420 (2550-2590)
302BS302158.0 (0.29)193 (28.0)16.2 (9.0)18.0 (10.0)19.4 (10.8)15.9 (9.2)21.6 (12.5)500 (0.12)7201.021375-1400 (2550-2550)
303S303008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)7201.021400-1450 (2550-2590)
304S304008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)7201.021400-1450 (2550-2650)
304LS304038.0 (0.29)————————1.021400-1450 (2550-2650)
302CuS304308.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)—11.2 (6.5)21.5 (12.4)500 (0.12)7201.021400-1450 (2550-2650)
304NS304518.0 (0.29)196 (28.5)—————500 (0.12)7201.021400-1450 (2550-2650)
305S305008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)7201.021400-1450 (2550-2650)
308S308008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)15.2 (8.8)21.6 (12.5)500 (0.12)720—1400-1420 (2550-2590)
309S309008.0 (0.29)200 (29.0)15.0 (8.3)16.6 (9.2)17.2 (9.6)15.6 (9.0)18.7 (10.8)500 (0.12)7801.021400-1450 (2550-2650)
310S310008.0 (0.29)200 (29.0)15.9 (8.8)16.2 (9.0)17.0 (9.4)14.2 (8.2)18.7 (10.8)500 (0.12)7801.021400-1450 (2550-2650)
314S314007.8 (0.28)200 (29.0)—15.1 (8.4)—17.5 (10.1)20.9 (12.1)500 (0.12)7701.02—
316S316008.0 (0.29)193 (28.0)15.9 (8.8)16.2 (9.0)17.5 (9.7)16.2 (9.4)21.5 (12.4)500 (0.12)7401.021375-1400 (2500-2550)
316LS316038.0 (0.29)————————1.021375-1400 (2500-2550)
316NS316518.0 (0.29)196 (28.5)—————500 (0.12)7401.021375-1400 (2500-2550)
317S317008.0 (0.29)193 (28.0)15.9 (8.8)16.2 (9.0)17.5 (9.7)16.2 (9.4)21.5 (12.4)500 (0.12)7401.021375-1400 (2500-2550)
317LS317038.0 (0.29)200 (29.0)16.5 (9.2)—18.1 (10.1)14.4 (8.3)—500 (0.12)790—1375-1400 (2500-2550)
321S321008.0 (0.29)193 (28.0)16.6 (9.2)17.2 (9.6)18.6 (10.3)16.1 (9.3)22.2 (12.8)500 (0.12)7201.021400-1425 (2550-2600)
329S329007.8 (0.28)——————460 (0.11)750——
330N083308.0 (0.29)196 (28.5)14.4 (8.0)16.0 (8.9)16.7 (9.3)——460 (0.11)10201.021400-1425 (2550-2600)
347S347008.0 (0.29)193 (28.0)16.6 (9.2)17.2 (9.6)18.6 (10.3)16.1 (9.3)22.2 (12.8)500 (0.12)7301.021400-1425 (2550-2600)
384S384008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)7901.021400-1450 (2550-2650)
405S405007.8 (0.28)200 (29.0)10.8 (6.0)11.6 (6.4)12.1 (6.7)27.0 (15.6)—460 (0.11)600—1480-1530 (2700-2790)
409S409007.8 (0.28)—11.7 (6.5)———————1480-1530 (2700-2790)
410S410007.8 (0.28)200 (29.0)9.9 (5.5)11.4 (6.3)11.6 (6.4)24.9 (14.4)28.7 (16.6)460 (0.11)570700-10001480-1530 (2700-2790)
414S414007.8 (0.28)200 (29.0)10.4 (5.8)11.0 (6.1)12.1 (6.7)24.9 (14.4)28.7 (16.6)460 (0.11)700—1425-1480 (2600-2700)
416S416007.8 (0.28)200 (29.0)9.9 (5.5)11.0 (6.1)11.6 (6.4)24.9 (14.4)28.7 (16.6)460 (0.11)570700-10001480-1530 (2700-2790)
420S420007.8 (0.28)200 (29.0)10.3 (5.7)10.8 (6.0)11.7 (6.5)24.9 (14.4)—460 (0.11)550—1450-1510 (2650-2750)
422S422007.8 (0.28)—11.2 (6.2)11.4 (6.3)11.9 (6.6)23.9 (13.8)27.3 (15.8)460 (0.11)——1470-1480 (2675-2700)
429S429007.8 (0.28)200 (29.0)10.3 (5.7)——25.6 (14.8)—460 (0.11)590—1450-1510 (2650-2750)
430S430007.8 (0.28)200 (29.0)10.4 (5.8)11.0 (6.1)11.4 (6.3)26.1 (15.1)26.3 (15.2)460 (0.11)600600-11001425-1510 (2600-2750)
430FS430207.8 (0.28)200 (29.0)10.4 (5.8)11.0 (6.1)11.4 (6.3)26.1 (15.1)26.3 (15.2)460 (0.11)600—1425-1510 (2600-2750)
431S431007.8 (0.28)200 (29.0)10.2 (5.7)12.1 (6.7)—20.2 (11.7)—460 (0.11)720——
434S434007.8 (0.28)200 (29.0)10.4 (5.8)11.0 (6.1)11.4 (6.3)—26.3 (15.2)460 (0.11)600600-11001425-1510 (2600-2750)
436S436007.8 (0.28)200 (29.0)9.3 (5.2)——23.9 (13.8)26.0 (15.0)460 (0.11)600600-11001425-1510 (2600-2750)
439S430357.7 (0.28)200 (29.0)10.4 (5.8)11.0 (6.1)11.4 (6.3)24.2 (14.0)—460 (0.11)630——
440AS440027.8 (0.28)200 (29.0)10.2 (5.7)——24.2 (14.0)—460 (0.11)600—1370-1480 (2500-2700)
440CS440047.8 (0.28)200 (29.0)10.2 (5.7)——24.2 (14.0)—460 (0.11)600—1370-1480 (2500-2700)
444S444007.8 (0.28)200 (29.0)10.0 (5.6)10.6 (5.9)11.4 (6.3)26.8 (15.5)—420 (0.10)620——
446S446007.5 (0.27)200 (29.0)10.4 (5.8)10.8 (6.0)11.2 (6.2)20.9 (12.1)24.4 (14.1)500 (0.12)670400-7001425-1510 (2600-2750)
PH 13-8 MoS138007.8 (0.28)203 (29.4)10.6 (5.9)11.2 (6.2)11.9 (6.6)14.0 (8.1)22.0 (12.7)460 (0.11)1020—1400-1440 (2560-2625)
15-5 PHS155007.8 (0.28)196 (28.5)10.8 (6.0)11.4 (6.3)—17.8 (10.3)23.0 (13.1)420 (0.10)770951400-1440 (2560-2625)
17-4 PHS174007.8 (0.28)196 (28.5)10.8 (6.0)11.6 (6.4)—18.3 (10.6)23.0 (13.1)460 (0.11)800951400-1440 (2560-2625)
17-7 PHS177007.8 (0.28)204 (29.5)11.0 (6.1)11.6 (6.4)—16.4 (9.5)21.8 (12.6)460 (0.11)830—1400-1440 (2560-2625)
  • (a) At 0 to 100 °C (32 to 212 °F).
  • (b) Approximate values.
  • CTE, coefficient of thermal expansion.

Stainless steel physical properties chart, printable PDF

All 48 grades with density, elastic modulus, thermal expansion, thermal conductivity, specific heat, electrical resistivity, magnetic permeability and melting range, in a printable PDF with our contact details.

Table notes

Typical physical properties of wrought stainless steels in the annealed condition: density, elastic modulus, mean coefficient of thermal expansion (CTE), thermal conductivity, specific heat, electrical resistivity, magnetic permeability and melting range. Values are given in metric units with the source’s imperial equivalents in parentheses.

CTE is the mean coefficient from 0 °C (32 °F) to the listed temperature; thermal conductivity is listed at 100 °C and 500 °C. These are the inputs used for thermal-expansion and heat-transfer calculations in tooling, dies and fixtures as well as for general design work.

Note: two melting ranges are printed inconsistently in the source and are reproduced as shown: type 302B, 1375–1400 °C (2550–2550 °F), and type 303, 1400–1450 °C (2550–2590 °F).

Magnetic permeability is an approximate value; the ferritic and martensitic types (405, 410, 420, 430, 440A, 440C, and others) are magnetic and the austenitic types are essentially non-magnetic (value 1.02). Verify against the applicable product specification before design use.

Stainless steel composition chart · Martensitic stainless steel mechanical properties · 420 stainless steel · 440C stainless steel · 440C stainless steel properties · 4Cr13 stainless steel · Stainless steels overview

Source: ASM Handbook, Volume 1 — Properties and Selection: Irons, Steels, and High-Performance Alloys, Table 21 “Typical physical properties of wrought stainless steels, annealed condition” (10th ed., pp. 2102–2106). Reference data for comparison — verify against the applicable product specification before design use.