스테인리스강 물리적 특성 차트

48종의 압연 스테인리스강(어닐링 상태) — 오스테나이트계, 페라이트계, 마르텐사이트계(410, 420, 440A, 440C) 및 석출경화계 — 의 밀도, 탄성계수, 열팽창, 열전도도, 비열, 전기저항 및 용융 범위. 미터법 수치와 영국식 환산값 제공.

유형UNS
번호
밀도
g/cm³
탄성
계수
GPa
0 °C (32 °F)에서부터의 평균 CTE열전도율비
열 (a)
J/kg·K
전기
저항률
nΩ·m
자석
투자율 (b)
용융 범위
°C (°F)
100 °C315 °C538 °C100 °C에서500 °C에서
201S201007.8 (0.28)197 (28.6)15.7 (8.7)17.5 (9.7)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)6901.021400-1450 (2550-2650)
202S202007.8 (0.28)—17.5 (9.7)18.4 (10.2)19.2 (10.7)16.2 (9.4)21.6 (12.5)500 (0.12)6901.021400-1450 (2550-2650)
205S205007.8 (0.28)197 (28.6)—17.9 (9.9)19.1 (10.6)——500 (0.12)———
301S301008.0 (0.29)193 (28.0)17.0 (9.4)17.2 (9.6)18.2 (10.1)16.2 (9.4)21.5 (12.4)500 (0.12)7201.021400-1420 (2550-2590)
302S302008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)7201.021400-1420 (2550-2590)
302BS302158.0 (0.29)193 (28.0)16.2 (9.0)18.0 (10.0)19.4 (10.8)15.9 (9.2)21.6 (12.5)500 (0.12)7201.021375-1400 (2550-2550)
303S303008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)7201.021400-1450 (2550-2590)
304S304008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)7201.021400-1450 (2550-2650)
304LS304038.0 (0.29)————————1.021400-1450 (2550-2650)
302CuS304308.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)—11.2 (6.5)21.5 (12.4)500 (0.12)7201.021400-1450 (2550-2650)
304NS304518.0 (0.29)196 (28.5)—————500 (0.12)7201.021400-1450 (2550-2650)
305S305008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)7201.021400-1450 (2550-2650)
308S308008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)15.2 (8.8)21.6 (12.5)500 (0.12)720—1400-1420 (2550-2590)
309S309008.0 (0.29)200 (29.0)15.0 (8.3)16.6 (9.2)17.2 (9.6)15.6 (9.0)18.7 (10.8)500 (0.12)7801.021400-1450 (2550-2650)
310S310008.0 (0.29)200 (29.0)15.9 (8.8)16.2 (9.0)17.0 (9.4)14.2 (8.2)18.7 (10.8)500 (0.12)7801.021400-1450 (2550-2650)
314S314007.8 (0.28)200 (29.0)—15.1 (8.4)—17.5 (10.1)20.9 (12.1)500 (0.12)7701.02—
316S316008.0 (0.29)193 (28.0)15.9 (8.8)16.2 (9.0)17.5 (9.7)16.2 (9.4)21.5 (12.4)500 (0.12)7401.021375-1400 (2500-2550)
316LS316038.0 (0.29)————————1.021375-1400 (2500-2550)
316NS316518.0 (0.29)196 (28.5)—————500 (0.12)7401.021375-1400 (2500-2550)
317S317008.0 (0.29)193 (28.0)15.9 (8.8)16.2 (9.0)17.5 (9.7)16.2 (9.4)21.5 (12.4)500 (0.12)7401.021375-1400 (2500-2550)
317LS317038.0 (0.29)200 (29.0)16.5 (9.2)—18.1 (10.1)14.4 (8.3)—500 (0.12)790—1375-1400 (2500-2550)
321S321008.0 (0.29)193 (28.0)16.6 (9.2)17.2 (9.6)18.6 (10.3)16.1 (9.3)22.2 (12.8)500 (0.12)7201.021400-1425 (2550-2600)
329S329007.8 (0.28)——————460 (0.11)750——
330N083308.0 (0.29)196 (28.5)14.4 (8.0)16.0 (8.9)16.7 (9.3)——460 (0.11)10201.021400-1425 (2550-2600)
347S347008.0 (0.29)193 (28.0)16.6 (9.2)17.2 (9.6)18.6 (10.3)16.1 (9.3)22.2 (12.8)500 (0.12)7301.021400-1425 (2550-2600)
384S384008.0 (0.29)193 (28.0)17.2 (9.6)17.8 (9.9)18.4 (10.2)16.2 (9.4)21.5 (12.4)500 (0.12)7901.021400-1450 (2550-2650)
405S405007.8 (0.28)200 (29.0)10.8 (6.0)11.6 (6.4)12.1 (6.7)27.0 (15.6)—460 (0.11)600—1480-1530 (2700-2790)
409S409007.8 (0.28)—11.7 (6.5)———————1480-1530 (2700-2790)
410S410007.8 (0.28)200 (29.0)9.9 (5.5)11.4 (6.3)11.6 (6.4)24.9 (14.4)28.7 (16.6)460 (0.11)570700-10001480-1530 (2700-2790)
414S414007.8 (0.28)200 (29.0)10.4 (5.8)11.0 (6.1)12.1 (6.7)24.9 (14.4)28.7 (16.6)460 (0.11)700—1425-1480 (2600-2700)
416S416007.8 (0.28)200 (29.0)9.9 (5.5)11.0 (6.1)11.6 (6.4)24.9 (14.4)28.7 (16.6)460 (0.11)570700-10001480-1530 (2700-2790)
420S420007.8 (0.28)200 (29.0)10.3 (5.7)10.8 (6.0)11.7 (6.5)24.9 (14.4)—460 (0.11)550—1450-1510 (2650-2750)
422S422007.8 (0.28)—11.2 (6.2)11.4 (6.3)11.9 (6.6)23.9 (13.8)27.3 (15.8)460 (0.11)——1470-1480 (2675-2700)
429S429007.8 (0.28)200 (29.0)10.3 (5.7)——25.6 (14.8)—460 (0.11)590—1450-1510 (2650-2750)
430S430007.8 (0.28)200 (29.0)10.4 (5.8)11.0 (6.1)11.4 (6.3)26.1 (15.1)26.3 (15.2)460 (0.11)600600-11001425-1510 (2600-2750)
430FS430207.8 (0.28)200 (29.0)10.4 (5.8)11.0 (6.1)11.4 (6.3)26.1 (15.1)26.3 (15.2)460 (0.11)600—1425-1510 (2600-2750)
431S431007.8 (0.28)200 (29.0)10.2 (5.7)12.1 (6.7)—20.2 (11.7)—460 (0.11)720——
434S434007.8 (0.28)200 (29.0)10.4 (5.8)11.0 (6.1)11.4 (6.3)—26.3 (15.2)460 (0.11)600600-11001425-1510 (2600-2750)
436S436007.8 (0.28)200 (29.0)9.3 (5.2)——23.9 (13.8)26.0 (15.0)460 (0.11)600600-11001425-1510 (2600-2750)
439S430357.7 (0.28)200 (29.0)10.4 (5.8)11.0 (6.1)11.4 (6.3)24.2 (14.0)—460 (0.11)630——
440AS440027.8 (0.28)200 (29.0)10.2 (5.7)——24.2 (14.0)—460 (0.11)600—1370-1480 (2500-2700)
440CS440047.8 (0.28)200 (29.0)10.2 (5.7)——24.2 (14.0)—460 (0.11)600—1370-1480 (2500-2700)
444S444007.8 (0.28)200 (29.0)10.0 (5.6)10.6 (5.9)11.4 (6.3)26.8 (15.5)—420 (0.10)620——
446S446007.5 (0.27)200 (29.0)10.4 (5.8)10.8 (6.0)11.2 (6.2)20.9 (12.1)24.4 (14.1)500 (0.12)670400-7001425-1510 (2600-2750)
PH 13-8 MoS138007.8 (0.28)203 (29.4)10.6 (5.9)11.2 (6.2)11.9 (6.6)14.0 (8.1)22.0 (12.7)460 (0.11)1020—1400-1440 (2560-2625)
15-5 PHS155007.8 (0.28)196 (28.5)10.8 (6.0)11.4 (6.3)—17.8 (10.3)23.0 (13.1)420 (0.10)770951400-1440 (2560-2625)
17-4 PHS174007.8 (0.28)196 (28.5)10.8 (6.0)11.6 (6.4)—18.3 (10.6)23.0 (13.1)460 (0.11)800951400-1440 (2560-2625)
17-7 PHS177007.8 (0.28)204 (29.5)11.0 (6.1)11.6 (6.4)—16.4 (9.5)21.8 (12.6)460 (0.11)830—1400-1440 (2560-2625)
  • (a) 0~100 °C (32~212 °F)에서.
  • (b) 근사값.
  • CTE, 열팽창 계수.

스테인리스 강 물리적 특성 차트, 인쇄 가능한 PDF

48개 등급의 밀도, 탄성계수, 열팽창, 열전도율, 비열, 전기 저항률, 투자율, 용융 범위를 담은 인쇄용 PDF입니다. 연락처가 함께 들어 있습니다.

테이블 노트

어닐링 상태의 단조 스테인리스강의 대표적 물리적 특성: 밀도, 탄성계수, 평균 열팽창계수(CTE), 열전도율, 비열, 전기저항률, 투자율 및 용융 범위. 값은 미터법 단위로 제시하며, 출처의 야드파운드법 환산값을 괄호 안에 병기합니다.

CTE는 0 °C (32 °F)에서 표기된 온도까지의 평균 계수이며, 열전도율은 100 °C 및 500 °C에서 표기됩니다. 이는 공구, 금형 및 지그의 열팽창 및 열전달 계산과 일반 설계 작업에 사용되는 입력값입니다.

메모: 출처에서 두 개의 용융 범위가 일관성 없이 인쇄되어 있으며 표기된 그대로 재현합니다: type 302B, 1375–1400 °C (2550–2550 °F), 및 type 303, 1400–1450 °C (2550–2590 °F).

자기 투자율은 근사값이며, 페라이트계 및 마르텐사이트계(405, 410, 420, 430, 440A, 440C 등)는 자성이 있고 오스테나이트계는 본질적으로 비자성(값 1.02)입니다. 설계 사용 전에 해당 제품 사양과 대조하여 확인하십시오.

스테인리스강 성분표 · 마르텐사이트계 스테인리스강 기계적 특성 · 420 스테인리스강 · 440C 스테인리스강 · 440C 스테인리스 강 특성 · 4Cr13 스테인리스강 · 스테인리스강 개요

출처: ASM Handbook, Volume 1 — Properties and Selection: Irons, Steels, and High-Performance Alloys, Table 21 “Typical physical properties of wrought stainless steels, annealed condition” (10th ed., pp. 2102–2106). 비교용 참조 데이터 — 설계에 사용하기 전에 해당 제품 사양과 대조하여 확인하십시오.