Stainless Steel Composition Chart

Chemical composition limits for the standard AISI stainless steel types — the austenitic, ferritic, duplex, martensitic and precipitation-hardening families. Ranges are in weight percent; a single value is a maximum unless marked “min”.

wt % all values

16.0-18.0 from–to range

0.15 min minimum content

0.045 maximum limit

— not specified

(a)–(b) footnote

TypeUNSCMnSiCrNiPSOther
Austenitic Types
201S201000.155.5-7.51.0016.0-18.03.5-5.50.060.030.25 N
202S202000.157.5-10.01.0017.0-19.04.0-6.00.060.030.25 N
205S205000.12-0.2514.0-15.51.0016.5-18.01.0-1.750.060.030.32-0.40 N
301S301000.152.001.0016.0-18.06.0-8.00.0450.03—
302S302000.152.001.0017.0-19.08.0-10.00.0450.03—
302BS302150.152.002.0-3.017.0-19.08.0-10.00.0450.03—
303S303000.152.001.0017.0-19.08.0-10.00.200.15 min0.6 Mo (b)
303SeS303230.152.001.0017.0-19.08.0-10.00.200.060.15 min Se
304S304000.082.001.0018.0-20.08.0-10.50.0450.03—
304HS304090.04-0.102.001.0018.0-20.08.0-10.50.0450.03—
304LS304030.032.001.0018.0-20.08.0-12.00.0450.03—
304LNS304530.032.001.0018.0-20.08.0-12.00.0450.030.10-0.16 N
302CuS304300.082.001.0017.0-19.08.0-10.00.0450.033.0-4.0 Cu
304NS304510.082.001.0018.0-20.08.0-10.50.0450.030.10-0.16 N
305S305000.122.001.0017.0-19.010.5-13.00.0450.03—
308S308000.082.001.0019.0-21.010.0-12.00.0450.03—
309S309000.202.001.0022.0-24.012.0-15.00.0450.03—
309SS309080.082.001.0022.0-24.012.0-15.00.0450.03—
310S310000.252.001.5024.0-26.019.0-22.00.0450.03—
310SS310080.082.001.5024.0-26.019.0-22.00.0450.03—
314S314000.252.001.5-3.023.0-26.019.0-22.00.0450.03—
316S316000.082.001.0016.0-18.010.0-14.00.0450.032.0-3.0 Mo
316FS316200.082.001.0016.0-18.010.0-14.00.200.10 min1.75-2.5 Mo
316HS316090.04-0.102.001.0016.0-18.010.0-14.00.0450.032.0-3.0 Mo
316LS316030.032.001.0016.0-18.010.0-14.00.0450.032.0-3.0 Mo
316LNS316530.032.001.0016.0-18.010.0-14.00.0450.032.0-3.0 Mo; 0.10-0.16 N
316NS316510.082.001.0016.0-18.010.0-14.00.0450.032.0-3.0 Mo; 0.10-0.16 N
317S317000.082.001.0018.0-20.011.0-15.00.0450.033.0-4.0 Mo
317LS317030.032.001.0018.0-20.011.0-15.00.0450.033.0-4.0 Mo
321S321000.082.001.0017.0-19.09.0-12.00.0450.035 × %C min Ti
321HS321090.04-0.102.001.0017.0-19.09.0-12.00.0450.035 × %C min Ti
330N083300.082.000.75-1.517.0-20.034.0-37.00.040.03—
347S347000.082.001.0017.0-19.09.0-13.00.0450.0310 × %C min Nb
347HS347090.04-0.102.001.0017.0-19.09.0-13.00.0450.038 × %C min – 1.0 max Nb
348S348000.082.001.0017.0-19.09.0-13.00.0450.030.2 Co; 10 × %C min Nb; 0.10 Ta
348HS348090.04-0.102.001.0017.0-19.09.0-13.00.0450.030.2 Co; 8 × %C min – 1.0 max Nb; 0.10 Ta
384S384000.082.001.0015.0-17.017.0-19.00.0450.03—
Ferritic types
405S405000.081.001.0011.5-14.5—0.040.030.10-0.30 Al
409S409000.081.001.0010.5-11.750.500.0450.0456 × %C min – 0.75 max Ti
429S429000.121.001.0014.0-16.0—0.040.03—
430S430000.121.001.0016.0-18.0—0.040.03—
430FS430200.121.251.0016.0-18.0—0.060.15 min0.6 Mo (b)
430FSeS430230.121.251.0016.0-18.0—0.060.060.15 min Se
434S434000.121.001.0016.0-18.0—0.040.030.75-1.25 Mo
436S436000.121.001.0016.0-18.0—0.040.030.75-1.25 Mo; 5 × %C min – 0.70 max Nb
439S430350.071.001.0017.0-19.00.500.040.030.15 Al; 12 × %C min – 1.10 Ti
442S442000.201.001.0018.0-23.0—0.040.03—
444S444000.0251.001.0017.5-19.51.000.040.031.75-2.50 Mo; 0.025 N; 0.2 + 4 (%C + %N) min – 0.8 max (Ti + Nb)
446S446000.201.501.0023.0-27.0—0.040.030.25 N
Duplex (ferritic-austenitic) type
329S329000.201.000.7523.0-28.02.50-5.000.0400.0301.00-2.00 Mo
Martensitic types
403S403000.151.000.5011.5-13.0—0.040.03—
410S410000.151.001.0011.5-13.5—0.040.03—
414S414000.151.001.0011.5-13.51.25-2.500.040.03—
416S416000.151.251.0012.0-14.0—0.060.15 min0.6 Mo (b)
416SeS416230.151.251.0012.0-14.0—0.060.060.15 min Se
420S420000.15 min1.001.0012.0-14.0—0.040.03—
420FS420200.15 min1.251.0012.0-14.0—0.060.15 min0.6 Mo (b)
422S422000.20-0.251.000.7511.5-13.50.5-1.00.040.030.75-1.25 Mo; 0.75-1.25 W; 0.15-0.3 V
431S431000.201.001.0015.0-17.01.25-2.500.040.03—
440AS440020.60-0.751.001.0016.0-18.0—0.040.030.75 Mo
440BS440030.75-0.951.001.0016.0-18.0—0.040.030.75 Mo
440CS440040.95-1.201.001.0016.0-18.0—0.040.030.75 Mo
Precipitation-hardening types
PH 13-8 MoS138000.050.200.1012.25-13.257.5-8.50.010.0082.0-2.5 Mo; 0.90-1.35 Al; 0.01 N
15-5 PHS155000.071.001.0014.0-15.53.5-5.50.040.032.5-4.5 Cu; 0.15-0.45 Nb
17-4 PHS174000.071.001.0015.5-17.53.0-5.00.040.033.0-5.0 Cu; 0.15-0.45 Nb
17-7 PHS177000.091.001.0016.0-18.06.5-7.750.040.040.75-1.5 Al
  • (a) Single values are maximum values unless otherwise indicated (a value followed by “min” is a minimum).
  • (b) Optional.

Table notes

The “Other” column gives additional specified elements — nitrogen, copper, titanium, niobium, aluminum, molybdenum, selenium and tungsten — as printed in the source.

Type 420 carbon is a minimum (0.15% min); actual carbon varies by heat, so check the mill certificate where hardness matters. UNS S30430 appears in this table under its AISI designation 302Cu; some references list the same composition as 304Cu.

Composition limits are heat analysis values from the source. Product analysis tolerances may apply — confirm the governing specification with your supplier before ordering.

Related reference pages

Stainless steels overview · 420 stainless steel · 420 stainless steel heat treatment · 440C stainless steel · 440C stainless steel properties · 440C stainless steel heat treatment · 4Cr13 stainless steel · 9Cr18Mo stainless steel · Tool steel composition chart · 95Cr18 (9Cr18) stainless steel · Stainless steel physical properties chart · Austenitic stainless mechanical properties

Source: ASM Handbook, Volume 1 — Properties and Selection: Irons, Steels, and High-Performance Alloys, Table 2 “Compositions of standard stainless steels” (10th ed.). Reference data for comparison — verify the applicable standard before ordering.