합금강 조성 차트

SAE-AISI 저합금 등급의 화학 조성 한도로, 용강 또는 주조 분석 기준 중량 퍼센트로 표기됩니다. 표는 13xx 망간 계열부터 40xx 몰리브덴, 41xx 크롬-몰리브덴, 43xx~48xx 니켈-크롬-몰리브덴, 51xx 크롬, 61xx 크롬-바나듐, 81xx~94xx 및 92xx 실리콘 등급까지 포함하며, SAE 잠재 표준 PS 등급은 두 번째 표에 있습니다.

wt % 용강 또는 주조 분석

빌릿, 블룸, 슬래브 및 열간 압연 또는 냉간 마감 봉강의 조성 한도. 판재에는 약간 더 넓은 범위가 적용됩니다. 출처의 표 19.

SAE-AISIUNSCMnPSSiNiCrMoV
1330G133000.28–0.331.60–1.900.0350.0400.15–0.35————
1335G133500.33–0.381.60–1.900.0350.0400.15–0.35————
1340G134000.38–0.431.60–1.900.0350.0400.15–0.35————
1345G134500.43–0.481.60–1.900.0350.0400.15–0.35————
4023G402300.20–0.250.70–0.900.0350.0400.15–0.35——
4024G402400.20–0.250.70–0.900.0350.035–0.0500.15–0.35——0.20–0.30—
4027G402700.25–0.300.70–0.900.0350.0400.15–0.35——0.20–0.30—
4028G402800.25–0.300.70–0.900.0350.035–0.0500.15–0.35——0.20–0.30—
4032G403200.30–0.350.70–0.900.0350.0400.15–0.35——0.20–0.30—
4037G403700.35–0.400.70–0.900.0350.0400.15–0.35——0.20–0.30—
4042G404200.40–0.450.70–0.900.0350.0400.15–0.35——0.20–0.30—
4047G404700.45–0.500.70–0.900.0350.0400.15–0.35——0.20–0.30—
4118G411800.18–0.230.70–0.900.0350.0400.15–0.35—0.40–0.600.08–0.15—
4130G413000.28–0.330.40–0.600.0350.0400.15–0.35—0.80–1.100.15–0.25—
4135G413500.33–0.380.70–0.900.0350.0400.15–0.35—0.80–1.100.15–0.25—
4137G413700.35–0.400.70–0.900.0350.0400.15–0.35—0.80–1.100.15–0.25—
4140G414000.38–0.430.75–1.000.0350.0400.15–0.35—0.80–1.100.15–0.25—
4142G414200.40–0.450.75–1.000.0350.0400.15–0.35—0.80–1.100.15–0.25—
4145G414500.41–0.480.75–1.000.0350.0400.15–0.35—0.80–1.100.15–0.25—
4147G414700.45–0.500.75–1.000.0350.0400.15–0.35—0.80–1.100.15–0.25—
4150G415000.48–0.530.75–1.000.0350.0400.15–0.35—0.80–1.100.15–0.25—
4161G416100.56–0.640.75–1.000.0350.0400.15–0.35—0.70–0.900.25–0.35—
4320G432000.17–0.220.45–0.650.0350.0400.15–0.351.65–2.000.40–0.600.20–0.30—
4340G434000.38–0.430.60–0.800.0350.0400.15–0.351.65–2.000.70–0.900.20–0.30—
E4340(b)G434060.38–0.430.65–0.850.0250.0250.15–0.351.65–2.000.70–0.900.20–0.30—
4422G442200.20–0.250.70–0.900.0350.0400.15–0.35——0.35–0.45—
4427G442700.24–0.290.70–0.900.0350.0400.15–0.35——0.35–0.45—
4615G461500.13–0.180.45–0.650.0350.0400.15–0.251.65–2.00—0.20–0.30—
4617G461700.15–0.200.45–0.650.0350.0400.15–0.351.65–2.00—0.20–0.30—
4620G462000.17–0.220.45–0.650.0350.0400.15–0.351.65–2.00—0.20–0.30—
4626G462600.24–0.290.45–0.650.035최대 0.040.15–0.350.70–1.00—0.15–0.25—
4718G471800.16–0.210.70–0.90———0.90–1.200.35–0.550.30–0.40—
4720G472000.17–0.220.50–0.700.0350.0400.15–0.350.90–1.200.35–0.550.15–0.25—
4815G481500.13–0.180.40–0.600.0350.0400.15–0.353.25–3.75—0.20–0.30—
4817G481700.15–0.200.40–0.600.0350.0400.15–0.353.25–3.75—0.20–0.30—
4820G482000.18–0.230.50–0.700.0350.0400.15–0.353.25–3.75—0.20–0.30—
50B40(c)G504010.38–0.430.75–1.000.0350.0400.15–0.35—0.40–0.60——
50B44(c)G504410.43–0.480.75–1.000.0350.0400.15–0.35—0.40–0.60——
5046G504600.43–0.480.75–1.000.0350.0400.15–0.35—0.20–0.35——
50B46(c)G504610.44–0.490.75–1.000.0350.0400.15–0.35—0.20–0.35——
50B50(c)G505010.48–0.530.75–1.000.0350.0400.15–0.35—0.40–0.60——
5060G506000.56–0.640.75–1.000.0350.0400.15–0.35—0.40–0.60——
50B60(c)G506010.56–0.640.75–1.000.0350.0400.15–0.35—0.40–0.60——
5115G511500.13–0.180.70–0.900.0350.0400.15–0.35—0.70–0.90——
5117G511700.15–0.200.70–0.900.0400.0400.15–0.35—0.70–0.90——
5120G512000.17–0.220.70–0.900.0350.0400.15–0.35—0.70–0.90——
5130G513000.28–0.330.70–0.900.0350.0400.15–0.35—0.80–1.10——
5132G513200.30–0.350.60–0.800.0350.0400.15–0.35—0.75–1.00——
5135G513500.33–0.380.60–0.800.0350.0400.15–0.35—0.80–1.05——
5140G514000.38–0.430.70–0.900.0350.0400.15–0.35—0.70–0.90——
5147G514700.46–0.510.70–0.950.0350.0400.15–0.35—0.85–1.15——
5150G515000.48–0.530.70–0.900.0350.0400.15–0.35—0.70–0.90——
5155G515500.51–0.590.70–0.900.0350.0400.15–0.35—0.70–0.90——
5160G516000.56–0.640.75–1.000.0350.0400.15–0.35—0.70–0.90——
51B60(c)G516010.56–0.640.75–1.000.0350.0400.15–0.35—0.70–0.90——
50100(b)G509860.98–1.100.25–0.450.0250.0250.15–0.35—0.40–0.60——
51100(b)G519860.98–1.100.25–0.450.0250.0250.15–0.35—0.90–1.15——
52100(b)G529860.98–1.100.25–0.450.0250.0250.15–0.35—1.30–1.60——
6118G611800.16–0.210.50–0.700.0350.0400.15–0.35—0.50–0.70—0.10–0.15
6150G615000.48–0.530.70–0.900.0350.0400.15–0.35—0.80–1.10—0.15 min
8115G811500.13–0.180.70–0.900.0350.0400.15–0.350.20–0.400.30–0.500.08–0.15—
81B45(c)G814510.43–0.480.75–1.000.0350.0400.15–0.350.20–0.400.35–0.550.08–0.15—
8615G861500.13–0.180.70–0.900.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8617G861700.15–0.200.70–0.900.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8620G862000.18–0.230.70–0.900.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8622G862200.20–0.250.70–0.900.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8625G862500.23–0.280.70–0.900.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8627G862700.25–0.300.70–0.900.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8630G863000.28–0.330.70–0.900.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8637G863700.35–0.400.75–1.000.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8640G864000.38–0.430.75–1.000.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8642G864200.40–0.450.75–1.000.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8645G864500.43–0.480.75–1.000.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
86B45(c)G864510.43–0.480.75–1.000.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8650G865000.48–0.530.75–1.000.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8655G865500.51–0.590.75–1.000.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8600G866000.56–0.640.75–1.000.0350.0400.15–0.350.40–0.700.40–0.600.15–0.25—
8720G872000.18–0.230.70–0.900.0350.0400.15–0.350.40–0.700.40–0.600.20–0.30—
8740G874000.38–0.430.75–1.000.0350.0400.15–0.350.40–0.700.40–0.600.20–0.30—
8822G882200.20–0.250.75–1.000.0350.0400.15–0.350.40–0.700.40–0.600.30–0.40—
9254G925400.51–0.590.60–0.800.0350.0401.20–1.60—0.60–0.80——
9260G926000.56–0.640.75–1.000.0350.0401.80–2.20————
9310(b)G931060.08–0.130.45–0.650.0250.0250.15–0.353.00–3.501.00–1.400.08–0.15—
94B15(c)G941510.13–0.180.75–1.000.0350.0400.15–0.350.30–0.600.30–0.500.08–0.15—
94B17(c)G941710.15–0.200.75–1.000.0350.0400.15–0.350.30–0.600.30–0.500.08–0.15—
94B30(c)G943010.28–0.330.75–1.000.0350.0400.15–0.350.30–0.600.30–0.500.08–0.15—

출처: ASM Handbook, Vol 1 (10th ed.), “Classification and Designation of Carbon and Low-Alloy Steels”, Table 19.

합금강 화학 성분표, 인쇄용 PDF

116개 강종의 화학 성분 한계, 망가니즈, 몰리브덴, 크롬, 니켈 계열과 SAE PS 강종, 원문 주석에 표시된 값, 연락처를 담은 A4 3페이지입니다. PDF는 영어로 제공됩니다.

SAE 잠재 표준강

PS 시리즈는 표준으로 제안된 등급으로, 화학 성분만이 아니라 경화능 요구 사항에 따라 공급되는 경우가 많습니다. 출처의 Table 20.

SAE PS 번호CMnP 최대S 최대SiNiCrMoB
PS 100.19–0.240.95–1.250.0350.0400.15–0.350.20–0.400.25–0.400.05–0.10—
PS 150.18–0.230.90–1.200.0350.0400.15–0.35—0.40–0.600.13–0.20—
PS 160.20–0.250.90–1.200.0350.0400.15–0.35—0.40–0.600.13–0.20—
PS 170.23–0.280.90–1.200.0350.0400.15–0.35—0.40–0.600.13–0.20—
PS 180.25–0.300.90–1.200.0350.0400.15–0.35—0.40–0.600.13–0.20—
PS 190.18–0.230.90–1.200.0350.0400.15–0.35—0.40–0.600.08–0.150.0005–0.003
PS 200.13–0.180.90–1.200.0350.0400.15–0.35—0.40–0.600.13–0.20—
PS 210.15–0.200.90–1.200.0350.0400.15–0.35—0.40–0.600.13–0.20—
PS 240.18–0.230.75–1.000.0350.0400.15–0.35—0.45–0.650.20–0.30—
PS 300.13–0.180.70–0.900.0350.0400.15–0.350.70–1.000.45–0.650.45–0.60—
PS 310.15–0.200.70–0.900.0350.0400.15–0.350.70–1.000.45–0.650.45–0.60—
PS 320.18–0.230.70–0.900.0350.0400.15–0.350.70–1.000.45–0.650.45–0.60—
PS 33(b)0.17–0.240.85–1.250.0350.0400.15–0.350.20 min0.20 min0.05 min—
PS 340.28–0.330.90–1.200.0350.0400.15–0.35—0.40–0.600.13–0.20—
PS 360.38–0.430.90–1.200.0350.0400.15–0.35—0.45–0.650.13–0.20—
PS 380.43–0.480.90–1.200.0350.0400.15–0.35—0.45–0.650.13–0.20—
PS 390.48–0.530.90–1.200.0350.0400.15–0.35—0.45–0.650.13–0.20—
PS 400.51–0.590.90–1.200.0350.0400.15–0.35—0.45–0.650.13–0.20—
PS 540.19–0.250.70–1.050.0350.0400.15–0.35—0.40–0.700.05 min—
PS 550.15–0.200.70–1.000.0350.0400.15–0.351.65–2.000.45–0.650.65–0.80—
PS 560.080–0.130.70–1.000.0350.0400.15–0.351.65–2.000.445–0.650.65–0.80—
PS 570.08 최대1.25 max0.0400.15–0.35최대 1.00—17.00–19.001.75–2.25—
PS 580.16–0.211.00–1.300.0350.0400.15–0.35—0.45–0.65——
PS 590.18–0.231.00–1.300.0350.0400.15–0.35—0.70–0.90——
PS 610.23–0.281.00–1.300.0350.0400.15–0.35—0.70–0.90——
PS 630.31–0.380.75–1.100.0350.0400.15–0.35—0.45–0.65—0.0005–0.003
PS 640.16–0.211.00–1.300.0350.0400.15–0.35—0.70–0.90——
PS 650.21–0.261.00–1.300.0350.0400.15–0.35—0.70–0.90——
PS 66(c)0.16–0.210.40–0.700.0350.0400.15–0.351.65–2.000.45–0.750.08–0.15—
PS 670.42–0.490.80–1.200.0350.0400.15–0.35—0.85–1.200.25–0.35—

출처: ASM Handbook, Vol 1 (10th ed.), “Classification and Designation of Carbon and Low-Alloy Steels”, Table 20.

합금강 화학 성분표, 인쇄용 PDF

116개 강종의 화학 성분 한계, 망가니즈, 몰리브덴, 크롬, 니켈 계열과 SAE PS 강종, 원문 주석에 표시된 값, 연락처를 담은 A4 3페이지입니다. PDF는 영어로 제공됩니다.

  • (a) 합금강에는 규정되거나 요구되지 않은 특정 원소가 소량 함유될 수 있습니다. 이러한 원소는 부수적인 것으로 간주되며 다음 최대치까지 허용됩니다. 구리 0.35%, 니켈 0.25%, 크롬 0.20%, 몰리브덴 0.06%.
  • (b) 전기로강이므로 E4340 행은 위의 4340 행보다 인과 황 함량이 낮습니다.
  • (c) 붕소 함량은 0.0005-0.003%입니다. 붕소는 합금 함량의 일부를 대체하여 경화능을 높이기 위해 첨가되며, 문자 B는 등급 번호의 마지막 두 자리 앞에 위치합니다.
  • (d) 일부 PS 강은 경화능 요구 사항에 따라 공급될 수 있습니다. PS 34와 PS 38은 J4에서 23-43 HRC 범위 내 15 HRC 포인트의 경화능 요구 사항으로 공급되며, PS 66은 바나듐 함량이 0.10-0.15%입니다.

테이블 노트

원본 표의 세 가지 값은 결함이 있는 상태로 인쇄되어 있습니다. 등급 4118의 몰리브덴은 0.08-015로 인쇄되어 있으며 여기서는 0.08-0.15로 표기합니다. 15% 몰리브덴 범위는 불가능하고 동일한 화학 조성이 표의 다른 곳에서 4118형 등급에 대해 올바르게 인쇄되어 있기 때문입니다. 등급 4023은 다른 모든 행이 미규정 표시를 가지고 있는 반면 몰리브덴 셀과 바나듐 셀이 비어 있으며, 해당 행은 인쇄된 그대로 재현됩니다. 등급 8600은 SAE 8660에 속하는 UNS 번호 G86600에 대해 인쇄되어 있으며, 해당 행은 번호를 다시 매기지 않고 인쇄된 그대로 재현됩니다. 두 가지 추가 값은 원본이 인쇄한 그대로 재현되었으며 특이해 보입니다. PS 56은 0.080-0.13% C와 0.445-0.65% Cr을 가지며, PS 57은 S max라는 열 제목 아래에 0.15-0.35% 황을 가집니다.

위 값은 중량 퍼센트 기준 레이들 또는 주조 분석 한계입니다. 제품 분석 공차는 더 넓으며 적용 표준에 의해 설정됩니다. 히트를 출하하기 전에 주문에 적용되는 한계를 재료 시험 성적서 또는 아오보 스틸과 확인하십시오.

조성 데이터는 일반 참고용입니다. 실제 값은 표준, 제철소 및 히트 번호에 따라 다릅니다. 재료 시험 성적서(MTC)와 확인하거나 아오보 스틸에 문의하십시오. 개별 강종에 대한 등급 페이지(예: 4140 조성는 하나의 등급에 대해 동일한 표 값을 열처리 및 응용 분야와 함께 제공합니다.

동일 등급에 두 가지 화학 조성이 있는 이유

위의 4340 행은 0.035% 인과 0.040% 황을 가집니다. 아래의 E4340 행은 0.025와 0.025를 가지는데, E는 더 깨끗한 잔류 수준의 전기로강을 나타내기 때문입니다. 둘 다 등급 번호에 대해 정확합니다.

붕소는 합금 함량을 절약합니다

붕소 등급은 더 적은 니켈, 크롬 및 몰리브덴으로 동일한 경화능에 도달합니다. 침탄강 가이드 는 침탄 부품에서 그 거래가 가치가 있는 시점을 제시합니다.

크롬과 몰리브덴이 역할을 합니다

41xx 계열에서 크롬은 경화능을 담당하고 몰리브덴은 뜨임 저항성을 담당합니다. 4140 특성 페이지 는 그 조합이 경도와 열처리에 미치는 영향을 보여줍니다.

히트 번호가 기재된 인증서를 요청하십시오

모든 합금강 출하품에는 히트 번호가 포함된 EN 10204 3.1 밀 인증서가 함께 제공되므로, 위의 한계값을 실제로 압연된 히트와 대조하여 확인할 수 있습니다.

탄소강 조성 차트 · 공구강 구성표 · 스테인리스강 성분표 · 4140 강재 특성 · 4340 강재 특성 · 8620 강재 특성 · 침탄강 가이드 · SCM415 합금강 · 강철 피삭성 등급 · H 강철 조성 차트

출처: ASM Handbook, Vol 1 (10th ed.), “Classification and Designation of Carbon and Low-Alloy Steels”, Tables 19 and 20. 값은 중량 퍼센트 기준 레이들 또는 주조 분석 한계입니다.