Bulk tool steel bar stock in the Aobo Steel warehouse

95Cr18 | 9Cr18 Stainless Steel

AOBO STEEL – Trusted Global Tool Steel Supplier

In China’s GB standards, 9Cr18 and 95Cr18 actually refer to the same type of steel. 95Cr18 is the new designation for 9Cr18 steel.

The old designation 9Cr18 originates from the GB/T 1220-1992 standard. It is primarily based on carbon and chromium content, with “9” representing a carbon content of approximately 0.9% and “18” representing a chromium content of approximately 18%.

The new grade 95Cr18 is named according to the latest GB/T 1220-2007 standard. The new naming convention is more standardized, with “95” representing a carbon content of approximately 0.95%, which more accurately indicates the carbon content compared to the old grade.

95Cr18 steel is a high-carbon, high-chromium martensitic stainless steel. It has high hardness, wear resistance, and corrosion resistance. This steel also exhibits good hot plasticity and low heat treatment deformation tendencies.

1. Chemical Composition(GB/T 1220—2007)

CSiMnCrSP
0.90% to 1.00%≤0.80%≤0.80%17.00% ~ 19.00%≤0.030%≤0.040%

For the improved version, “9Cr18Mo” (also known as AISI 440C), the composition includes Molybdenum (Mo) typically in the range of 0.40% to 0.70%.

2. Physical Properties of 95Cr18(9Cr18)

Critical Point Temperature

Critical PointTemperature (approximate) / °C
Ac₁830
Ar₁810

Linear Expansion Coefficient

Temperature / °CLinear Expansion Coefficient α / (10⁻⁶ °C⁻¹)
20 ~ 10010.5
20 ~ 20011
20 ~ 30011
20 ~ 40011.5
20 ~ 50012

Other Physical Properties

PropertyValue
Density / (g/cm³)7.7
Modulus of Elasticity E(20°C) / MPa203,890
Specific Heat Capacity cₚ(20°C) / [J/(kg·K)]459.8
Thermal Conductivity λ(20°C) / [W/(m·K)]29.3
Electrical Resistivity ρ(20°C) / (10⁻⁶ Ω·m)0.6
95Cr18 Stainless Steel
95Cr18 Stainless Steel

Are you looking for a 9Cr18 Stainless Steel supplier? Please fill out the form below to contact us today!

    3. Forging Process of 95Cr18(9Cr18)

    Furnace Charging TemperatureInitial Forging Temperature / °CFinal Forging Temperature / °CCooling
    Cold charging temp. ≤600°C, Hot charging temp. unlimited1050 ~ 1100≥850Furnace cooling

    Note: The heating speed of the hot working process should not be too fast. The stop forging (rolling) temperature should be controlled at a higher level, and slow cooling conditions must be strictly followed.

    4. Heat Treatment of 95Cr18(9Cr18)

    4.1 Preliminary Heat Treatment Specification of 95Cr18 Steel

    Preliminary Heat Treatment PlanHeating Temperature / °CCooling MethodHardness HBW
    Softening Annealing800 ~ 840Furnace cool to 500°C, then air cool≤255¹
    Full Annealing840 ~ 860Furnace cooling≤255¹

    Note: ① The annealed structure is pearlite.

    4.2 Quenching and Tempering

    4.2.1 Quenching and Tempering Process Specification of 95Cr18 Steel

    Quenching Temp. / °CCooling MethodHardness HRC (Quenching)Tempering Temp. / °CHardness HRC (Tempering)
    1030 ~ 1070Oil cooling≥55200 ~ 30056

    4.2.2 Hardness, Retained Austenite Content, and Impact Toughness

    Quenching Temp. / °CHardness HRCRetained Austenite (vol. fraction, %)aₖ / (J/cm²)
    80035—31
    90048—17
    950521.714
    1000575.211
    10506029.210
    11005393.915
    1150429722
    1200359926

    4.2.3 Effect of Different Tempering Temperatures on Hardness and Impact Toughness

    Tempering Temp. / °CAfter Quenching100200300400450500550600650
    Hardness HRC60605855565754474032
    aₖ / (J/cm²)11.52028292422212530—

    4.3 Cold Treatment

    4.3.1 Cold Treatment Process Specification

    Cold Treatment ProcessHardness HBW
    1000°C × 10min + -73°C × 6-8h + 100-200°C × 30-40min Air Cooling55 ~ 60

    4.3.2 Effect of Cold Treatment on the Hardness

    Quenching Temperature/°CHardness HRCHardness HRC after cooling to -75°C and holding for 1hHardness HRC after Tempering (Tempering Temperature)
    100°C150°C200°C
    100058—585755
    10005959.559.55957
    10506061.5616159
    110060.562626260.5

    5. Corrosion Resistance of 95Cr18 (9Cr18) Steel

    MediumMass Fraction (%)Temperature/℃Corrosion Rate /mm⋅a-1
    Nitric acid5 – 2020< 0.1
    560 ~ Boiling< 1.0
    2060< 0.1
    2080< 1.0
    20Boiling2.0 ~ 3.0
    4060 ~ 80< 1.0
    40Boiling3.0 ~ 10.0
    5020< 0.1
    5080< 1.0
    6020< 0.1
    6060 ~ 80< 1.0
    60Boiling1.0 ~ 3.0
    9020< 1.0
    90Boiling3.0 ~ 10.0
    Acetic acid520< 1.0
    550 ~ 753.0 ~ 10.0
    5Boiling> 10.0
    2550 ~ 753.0 ~ 10.0
    25Boiling> 10.0
    5020< 0.1
    50503.0 ~ 10.0
    5075> 10.0
    Phosphoric acid120< 0.1
    1020< 3.0
    15203.0 ~ 10.0
    Sulfuric acid520> 10.0
    550> 10.0
    580> 10.0
    Hydrochloric acid0.520< 1.0
    0.550< 3.0
    0.5Boiling> 10.0
    120< 3.0
    1503.0 ~ 10.0

    Your Premier Source for 9Cr18 Stainless Steel

    Leverage our 20+ years of expertise. We supply top-grade 9Cr18 stainless steel, ideal for high-wear and corrosion-resistant applications. Contact our specialists for detailed specifications and a competitive quote.

    Expert Guidance
    Market-Leading Prices