Mechanical Properties of Austenitic Stainless Steels
Minimum room-temperature tensile and yield strength, elongation, reduction in area and hardness for the wrought austenitic stainless steels, quoted for each product form and condition with the ASTM specification that carries the requirement. A minimum is the floor a heat has to clear, so a certificate usually shows more.
The minimum values each product form and condition is required to meet, with the ASTM specification that carries the requirement. Table 7 of the source.
| Type | UNS | Form | Condition | Tensile MPa | Tensile ksi | Yield 0.2% MPa | Yield 0.2% ksi | Elong. % | Red. of area, % | Hardness HRB | ASTM |
|---|---|---|---|---|---|---|---|---|---|---|---|
| Type 301 | S30100 | B | Annealed | 620 | 90 | 205 | 30 | 40 | — | 95 max | A 666 |
| Type 301 | S30100 | B, P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 92 max | A 167 |
| Type 301 | S30100 | B, P, Sh, St | 1/4 hard | 860 | 125 | 515 | 75 | 25 | — | — | A 666 |
| Type 301 | S30100 | B, P, Sh, St | 1/2 hard | 1030 | 150 | 760 | 110 | 18 | — | — | A 666 |
| Type 301 | S30100 | B, P, Sh, St | 3/4 hard | 1210 | 175 | 930 | 135 | 12 | — | — | A 666 |
| Type 301 | S30100 | B, P, Sh, St | Full hard | 1280 | 185 | 965 | 140 | 9 | — | — | A 666 |
| Type 302 | S30200 | B, F | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276, A 473 |
| Type 302 | S30200 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 302 | S30200 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Type 302 | S30200 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Type 302 | S30200 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 302 | S30200 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 92 max | A 167, A 240, A 666 |
| Type 302 | S30200 | B, P, Sh, St | High tensile, 1/4 hard | 860 | 125 | 515 | 75 | 10 | — | — | A 666 |
| Type 302 | S30200 | B, P, Sh, St | High tensile, 1/2 hard | 1030 | 150 | 760 | 110 | 10 | — | — | A 666 |
| Type 302 | S30200 | B, P, Sh, St | High tensile, 3/4 hard | 1205 | 175 | 930 | 135 | 6 | — | — | A 666 |
| Type 302 | S30200 | B, P, Sh, St | Full hard | 1275 | 185 | 965 | 140 | 4 | — | — | A 666 |
| Type 302B | S30215 | B, F | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276, A 473 |
| Type 302B | S30215 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 302B | S30215 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Type 302B | S30215 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Type 302B | S30215 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 302B | S30215 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 95 max | A 167 |
| Type 302Cu | S30430 | W(e) | Annealed | 550 | 80 | — | — | — | — | — | A 493 |
| Type 302Cu | S30430 | W(e) | Lightly drafted | 585 | 85 | — | — | — | — | — | A 493 |
| Types 303 and 303Se | S30300, S30323 | F | Annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 473 |
| Types 303 and 303Se | S30300, S30323 | W | Annealed | 585–860 | 85–125 | — | — | — | — | — | A 581 |
| Types 303 and 303Se | S30300, S30323 | W | Cold worked | 790–1000 | 115–145 | — | — | — | — | — | A 581 |
| Type 304 | S30400 | B, F(f) | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276, A 473 |
| Type 304 | S30400 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 304 | S30400 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Type 304 | S30400 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Type 304 | S30400 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 304 | S30400 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 92 max | A 167 |
| Type 304 | S30400 | B, P, Sh, St | 1/8 hard | 690 | 100 | 380 | 55 | 35 | — | — | A 666 |
| Type 304 | S30400 | B, P, Sh, St | 1/4 hard | 860 | 125 | 515 | 75 | 10 | — | — | A 666 |
| Type 304 | S30400 | B, P, Sh, St | 1/2 hard | 1035 | 150 | 760 | 110 | 7 | — | — | A 666 |
| Type 304L | S30403 | F | Annealed | 450 | 65 | 170 | 25 | 40 | 50 | — | A 473 |
| Type 304L | S30403 | B | Hot finished and annealed | 480 | 70 | 170 | 25 | 40 | 50 | — | A 276 |
| Type 304L | S30403 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 304L | S30403 | B | Cold finished(c) and annealed | 480 | 70 | 170 | 25 | 30 | 40 | — | A 276 |
| Type 304L | S30403 | W | Annealed | 480 | 70 | 170 | 25 | 35(d) | 50(d) | — | A 580 |
| Type 304L | S30403 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 304L | S30403 | P, Sh, St | Annealed | 480 | 70 | 170 | 25 | 40 | — | 88 max | A 167, A 240 |
| Type 304B4 | S30424 | P, Sh, St grade A | Annealed | 515 | 75 | 205 | 30 | 27 | — | 95 max | A 887 |
| Type 304B4 | S30424 | P, Sh, St grade B | Annealed | 515 | 75 | 205 | 30 | 16 | — | 95 max | A 887 |
| Type 305 | S30500 | B, F | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276, A 473 |
| Type 305 | S30500 | B | Cold finished(b) and annealed | 260 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 305 | S30500 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Type 305 | S30500 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Type 305 | S30500 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 305 | S30500 | P, Sh, St | Annealed | 480 | 70 | 170 | 25 | 40 | — | 88 max | A 167 |
| Type 305 | S30500 | B, W | High tensile(d) | 1690 | 245 | — | — | — | — | — | — |
| Cronifer 18-15 LCSi | S30600 | P, Sh, St | Annealed | 540 | 78 | 240 | 35 | 40 | — | — | A 167, A 240 |
| Type 308 | S30800 | B, F | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276, A 473 |
| Type 308 | S30800 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 308 | S30800 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Type 308 | S30800 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Type 308 | S30800 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 308 | S30800 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 88 max | A 167 |
| Types 309, 309S, 310 and 310S | S30900, S30908, S31000, S31008 | B, F | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276, A 473 |
| Types 309, 309S, 310 and 310S | S30900, S30908, S31000, S31008 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Types 309, 309S, 310 and 310S | S30900, S30908, S31000, S31008 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Types 309, 309S, 310 and 310S | S30900, S30908, S31000, S31008 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Types 309, 309S, 310 and 310S | S30900, S30908, S31000, S31008 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Types 309, 309S, 310 and 310S | S30900, S30908, S31000, S31008 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 95 max | A 167 |
| 310Cb | S31040 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 95 | A 167, A 240 |
| 310Cb | S31040 | B, Shapes | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276 |
| 310Cb | S31040 | B, Shapes | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| 310Cb | S31040 | B, Shapes | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| 310Cb | S31040 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| 310Cb | S31040 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 314 | S31400 | B, F | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276, A 473 |
| Type 314 | S31400 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 314 | S31400 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Type 314 | S31400 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Type 314 | S31400 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 316 | S31600 | B, F(f) | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276, A 473 |
| Type 316 | S31600 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 316 | S31600 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Type 316 | S31600 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | — |
| Type 316 | S31600 | W | Cold finished | 620 | 90 | 310 | 45 | 40(d) | 40 | — | A 580 |
| Type 316 | S31600 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 95 max | A 167, A 240 |
| Type 316L | S31603 | F | Annealed | 450 | 65 | 170 | 25 | 40 | 50 | — | A 473 |
| Type 316L | S31603 | B | Hot finished and annealed | 480 | 70 | 170 | 25 | 40 | 50 | — | A 276 |
| Type 316L | S31603 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 316L | S31603 | B | Cold finished(c) and annealed | 480 | 70 | 170 | 25 | 30 | 40 | — | A 276 |
| Type 316L | S31603 | W | Annealed | 480 | 70 | 170 | 25 | 35(d) | 50(d) | — | A 580 |
| Type 316L | S31603 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 316L | S31603 | P, Sh, St | Annealed | 485 | 70 | 170 | 25 | 40 | — | 95 max | A 167, A 240 |
| Type 316Cb | S31640 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 30 | — | 95 | A 167, A 240 |
| Type 316Cb | S31640 | B, Shapes | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276 |
| Type 316Cb | S31640 | B, Shapes | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 316Cb | S31640 | B, Shapes | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Type 316Cb | S31640 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Type 316Cb | S31640 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 317 | S31700 | B, F | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276, A 473 |
| Type 317 | S31700 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Type 317 | S31700 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Type 317 | S31700 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Type 317 | S31700 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Type 317 | S31700 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 35 | — | 95 max | A 167, A 240 |
| Type 317L | S31703 | B | Annealed | 585(g) | 85(g) | 240(g) | 35(g) | 55(g) | 65(g) | 85 max(g) | — |
| Type 317L | S31703 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 95 max | A 167 |
| Type 317LM | S31725 | B, P | Annealed | 515 | 75 | 205 | 30 | 40 | — | — | A 276 |
| Type 317LM | S31725 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 95 max | A 167 |
| Types 321 and 321H | S32100, S32109 | B, F | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | — | A 276, A 473 |
| Types 321 and 321H | S32100, S32109 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Types 321 and 321H | S32100, S32109 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Types 321 and 321H | S32100, S32109 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Types 321 and 321H | S32100, S32109 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Types 321 and 321H | S32100, S32109 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 95 max | A 167, A 240 |
| Types 347 and 348 | S34700, S34800 | B, F | Hot finished and annealed | 515 | 75 | 205 | 30 | 40 | 50 | A 276, A 473 | |
| Types 347 and 348 | S34700, S34800 | B | Cold finished(b) and annealed | 620 | 90 | 310 | 45 | 30 | 40 | — | A 276 |
| Types 347 and 348 | S34700, S34800 | B | Cold finished(c) and annealed | 515 | 75 | 205 | 30 | 30 | 40 | — | A 276 |
| Types 347 and 348 | S34700, S34800 | W | Annealed | 515 | 75 | 205 | 30 | 35(d) | 50(d) | — | A 580 |
| Types 347 and 348 | S34700, S34800 | W | Cold finished | 620 | 90 | 310 | 45 | 30(d) | 40 | — | A 580 |
| Types 347 and 348 | S34700, S34800 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 92 max | A 167, A 240 |
| 18-18-2 | S38100 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 95 max | A 167, A 240 |
| Type 384 | S38400 | W(e) | Annealed | 550 | 80 | — | — | — | — | — | A 493 |
| Type 384 | S38400 | W(e) | Lightly drafted | 585 | 85 | — | — | — | — | — | A 493 |
| 20Cb-3, 20Mo-4, and 20Mo-6 | N08020, N08024, N08026 | B, W | Annealed | 550 | 80 | 240 | 35 | 30 | 50 | — | B 473 |
| 20Cb-3, 20Mo-4, and 20Mo-6 | N08020, N08024, N08026 | Shapes | Annealed | 550 | 80 | 240 | 35 | 15 | 50 | — | B 473 |
| 20Cb-3, 20Mo-4, and 20Mo-6 | N08020, N08024, N08026 | B, W | Annealed and strain hardened | 620 | 90 | 415 | 60 | 15 | 40 | — | B 473 |
| 20Cb-3, 20Mo-4, and 20Mo-6 | N08020, N08024, N08026 | W | Annealed and cold finished | 620–830 | 90–120 | — | — | — | — | — | B 473 |
| 20Cb-3, 20Mo-4, and 20Mo-6 | N08020, N08024, N08026 | P, Sh, St | Annealed | 550 | 80 | 240 | 35 | 30 | — | 95 max | B 463 |
| 20Cb-3, 20Mo-4, and 20Mo-6 | N08020, N08024, N08026 | Pi, T | Annealed | 550 | 80 | 240 | 35 | 30 | — | — | B 464, B 468, B 474, B 729 |
| Sanicro 28 | N08028 | P, Sh, St | Annealed | 500 | 73 | 215 | 31 | 40 | — | 70-90(g) | B 709 |
| Sanicro 28 | N08028 | Seamless Tube | Annealed | 500 | 73 | 215 | 31 | 40 | — | — | B 668 |
| Type 330 | N08330 | B | Annealed | 485 | 70 | 210 | 30 | 30 | — | — | B 511 |
| Type 330 | N08330 | P, Sh, St | Annealed | 485 | 70 | 210 | 30 | 30 | — | 70-90(g) | B 536 |
| Type 330 | N08330 | Pi | Annealed | 485 | 70 | 210 | 30 | 30 | — | 70-90(g) | B 535, B 546 |
| AL-6X | N08366 | B, W | Annealed | 515 | 75 | 210 | 30 | 30 | — | — | B 691 |
| AL-6X | N08366 | P, Sh, St | Annealed | 515 | 75 | 240 | 35 | 30 | — | 95 max | B 688 |
| AL-6X | N08366 | Pi, T | Annealed | 515 | 75 | 210 | 30 | 30 | — | — | B 675, B 676, B 690 |
| AL-6X | N08366 | Welded T | Cold worked | 515 | 75 | 210 | 30 | 10 | — | — | B 676 |
| JS-700 | N08700 | B, W | Annealed | 550 | 80 | 240 | 35 | 30 | 50 | — | B 672 |
| JS-700 | N08700 | P, Sh, St | Annealed | 550 | 80 | 240 | 35 | 30 | — | 75-90(g) | B 599 |
| Type 332 | N08800 | Pi, T | Annealed | 515 | 75 | 210 | 30 | 30 | — | — | B 163, B 407, B 514, B 515 |
| Type 332 | N08800 | Seamless Pi, T | Hot finished | 450 | 65 | 170 | 25 | 30 | — | — | B 407 |
| Type 332 | N08800 | B | Hot worked | 550 | 80 | 240 | 35 | 25 | — | — | B 408 |
| Type 332 | N08800 | B | Annealed | 515 | 75 | 210 | 30 | 30 | — | — | B 408 |
| Type 332 | N08800 | P | Hot rolled | 550 | 80 | 240 | 35 | 25 | — | — | B 409 |
| Type 332 | N08800 | P, Sh, St | Annealed | 515 | 75 | 210 | 30 | 30 | — | — | B 409 |
| Type 904L | N08904 | B | Annealed | 490 | 71 | 220 | 31 | 35 | — | — | B 649 |
| Type 904L | N08904 | W | Cold finished | 620–830 | 90–120 | — | — | — | — | — | B 649 |
| Type 904L | N08904 | Pi, T | Annealed | 490 | 71 | 220 | 31 | 35 | — | — | B 673, B 674, B 677 |
| Type 904L | N08904 | P, Sh, St | Annealed | 490 | 71 | 220 | 31 | 35 | — | 70-90(g) | B 625 |
Source: ASM Handbook, Vol 1 (10th ed.), “Wrought Stainless Steels”, Table 7.
Austenitic stainless mechanical properties, printable PDF
Three A4 pages with the minimum tensile and yield strengths, elongation, reduction of area and hardness for 147 type, form and condition rows, the ASTM specification named in each row, and our contact details.
- (a) B, bar; F, forgings; P, plate; Pi, pipe; Sh, sheet; St, strip; T, tube; W, wire.
- (b) Up to 13 mm (0.5 in.) thick.
- (c) Over 13 mm (0.5 in.) thick.
- (d) For wire 3.96 mm (5/32 in.) and under, elongation and reduction in area shall be 25 and 40%, respectively.
- (e) 4 mm (0.156 in.) in diameter and over.
- (f) For forged sections 127 mm (5 in.) and over, the tensile strength shall be 485 MPa (70 ksi).
- (g) For information only, not a basis for acceptance or rejection.
High-nitrogen austenitic stainless steels
The high-nitrogen grades, where nitrogen replaces part of the nickel for strength and for resistance to pitting. Table 8 of the source.
| Type | UNS | Form | Condition | Tensile MPa | Tensile ksi | Yield 0.2% MPa | Yield 0.2% ksi | Elong. % | Red. of area, % | Hardness HRB | ASTM |
|---|---|---|---|---|---|---|---|---|---|---|---|
| Type 201 | S20100 | B | Annealed | 515 | 75 | 275 | 40 | 40 | 45 | — | A 276 |
| Type 201 | S20100 | P, Sh, St | Annealed | 655 | 95 | 310 | 45 | 40 | — | 100 max | A 276, A 666 |
| Type 201 | S20100 | Sh, St | 1/4 hard | 860 | 125 | 515 | 75 | 25 | — | — | A 666 |
| Type 201 | S20100 | Sh, St | 1/2 hard | 1030 | 150 | 760 | 110 | 18 | — | — | A 666 |
| Type 201 | S20100 | Sh, St | 3/4 hard | 1210 | 175 | 930 | 135 | 12 | — | — | A 666 |
| Type 201 | S20100 | Sh, St | Full hard | 1280 | 185 | 965 | 140 | 9 | — | — | A 666 |
| Type 202 | S20200 | B | Annealed | 515 | 75 | 275 | 40 | 40 | 45 | — | A 276 |
| Type 202 | S20200 | P, Sh, St | Annealed | 620 | 90 | 260 | 38 | 40 | — | — | A 666 |
| Type 202 | S20200 | Sh, St | 1/4 hard | 860 | 125 | 515 | 75 | 12 | — | — | A 660 |
| Type 205 | S20500 | B, P, Sh, St | Annealed | 790 | 115 | 450 | 65 | 40 | — | 10 max | A 666 |
| Nitronic 50 | S20910 | B | Annealed | 690 | 100 | 380 | 55 | 35 | 55 | — | A 276 |
| Nitronic 50 | S20910 | W | Annealed | 690 | 100 | 380 | 55 | 35 | 55 | — | A 580 |
| Nitronic 50 | S20910 | Sh, St | Annealed | 725 | 105 | 415 | 60 | 30 | — | 100 max | A 240 |
| Nitronic 50 | S20910 | P | Annealed | 690 | 100 | 380 | 55 | 35 | — | 100 max | A 240 |
| Cryogenic Tenelon | S21460 | B, P, Sh, St | Annealed | 725 | 105 | 380 | 55 | 40 | — | — | A 666 |
| Types 216 and 216L | S21600, S21603 | Sh, St | Annealed | 690 | 100 | 415 | 60 | 40 | — | 100 max | A 240 |
| Types 216 and 216L | S21600, S21603 | P | Annealed | 620 | 90 | 345 | 50 | 40 | — | 100 max | A 240 |
| Nitronic 40 | S21900 | B, W | Annealed | 620 | 90 | 345 | 50 | 45 | 60 | — | A 276, A 580 |
| 21-6-9 LC (XM-11) | S21904 | B, W, shapes | Annealed | 620 | 90 | 345 | 50 | 45 | 60 | — | A 276, A 580 |
| 21-6-9 LC (XM-11) | S21904 | Sh, St | Annealed | 690 | 100 | 415 | 60 | 40 | — | — | A 666 |
| 21-6-9 LC (XM-11) | S21904 | P | Annealed | 620 | 90 | 345 | 50 | 45 | — | — | A 666 |
| Nitronic 33 | S24000 | B, W | Annealed | 690 | 100 | 380 | 55 | 30 | 50 | — | A 276, A 580 |
| Nitronic 33 | S24000 | Sh, St | Annealed | 690 | 100 | 415 | 60 | 40 | — | 100 max | A 240 |
| Nitronic 33 | S24000 | P | Annealed | 690 | 100 | 380 | 55 | 40 | — | 100 max | A 240 |
| Nitronic 32 | S24100 | B, W | Annealed | 690 | 100 | 380 | 55 | 30 | 50 | — | A 276, A 580 |
| Type 304N | S30451 | B | Annealed | 550 | 80 | 240 | 35 | 30 | — | — | A 276 |
| Type 304N | S30451 | P, Sh, St | Annealed | 550 | 80 | 240 | 35 | 30 | — | 92 max | A 240 |
| Type 340HN | S30452 | B | Annealed | 620 | 90 | 345 | 50 | 30 | 50 | — | A 276 |
| Type 340HN | S30452 | Sh, St | Annealed | 620 | 90 | 345 | 50 | 30 | — | 100 max | A 240 |
| Type 340HN | S30452 | P | Annealed | 585 | 85 | 275 | 40 | 30 | — | 100 max | A 240 |
| Type 304LN | S30453 | B | Annealed | 515 | 75 | 205 | 30 | — | — | — | A 276 |
| Type 304LN | S30453 | P, Sh, St | Annealed | 515 | 75 | 205 | 30 | 40 | — | 92 max | A 167, A 240 |
| 253 MA | S30815 | P, Sh, St | Annealed | 600 | 87 | 310 | 45 | 40 | — | 95 max | A 167, A 240 |
| 253 MA | S30815 | B, shapes | Annealed | 600 | 87 | 310 | 45 | 40 | 50 | — | A 276 |
| 254 SMO | S31254 | P, Sh, St | Annealed | 650 | 94 | 300 | 44 | 35 | — | 96 | A 167, A 240 |
| 254 SMO | S31254 | B, shapes | Annealed | 650 | 95 | 300 | 44 | 35 | 50 | — | A 276 |
| Type 316N | S31651 | B | Annealed | 550 | 80 | 240 | 35 | 30 | — | — | A 276 |
| Type 316N | S31651 | P, Sh, St | Annealed | 550 | 80 | 240 | 35 | 35 | — | 95 max | A 240 |
| 17-14-4 LN | S31726 | P, Sh, St | Annealed | 550 | 80 | 240 | 35 | 40 | — | 96 | A 167, A 240 |
| 17-14-4 LN | S31726 | B, shapes | Annealed | 550 | 80 | 240 | 35 | 40 | — | — | A 276 |
| 317LN | S31753 | P, Sh, St | Annealed | 550 | 80 | 240 | 35 | 40 | — | 95 | A 167, A 240 |
| AL 6XN | N08367 | B, W | Annealed | 715 | 104 | 315 | 46 | 30 | — | — | B691 |
| AL 6XN | N08367 | P, Sh, St | Annealed | 715 | 104 | 315 | 46 | 30 | — | 100 | B688 |
| AL 6XN | N08367 | Flanges, fittings, valves, and so on | Annealed | 715 | 104 | 315 | 46 | 30 | 50 | — | B462 |
| AL 6XN | N08367 | Seamless Pi, T | Annealed | 715 | 104 | 315 | 46 | 30 | — | — | B690 |
| AL 6XN | N08367 | Welded Pi | Annealed | 715 | 104 | 315 | 46 | 30 | — | — | B676 |
| AL 6XN | N08367 | Welded T | Solution treated and annealed | 715 | 104 | 315 | 46 | 30 | — | — | B676 |
| AL 6XN | N08367 | Welded T | Cold worked | — | — | — | — | 10 | — | — | B676 |
| Cronifer 1925 hMO | N08925 | B, W | Annealed | 600 | 87 | 300 | 43 | 40 | — | — | B649 |
| Cronifer 1925 hMO | N08925 | Seamless Pi, T | Annealed | 600 | 87 | 300 | 43 | 40 | — | — | B677 |
| Cronifer 1925 hMO | N08925 | Welded Pi | Annealed | 600 | 87 | 300 | 43 | 40 | — | — | B673 |
| Cronifer 1925 hMO | N08925 | Welded T | Annealed | 600 | 87 | 300 | 43 | 40 | — | — | B674 |
Source: ASM Handbook, Vol 1 (10th ed.), “Wrought Stainless Steels”, Table 8. Values are minimum room-temperature properties by product form and condition.
- (a) B, bar; P, plate; Pi, pipe; Sh, sheet; St, strip; T, tube; W, wire.
- Product form codes are B for bar, P for plate, Sh for sheet, St for strip, and W for wire. A type can carry different minimums in different forms, which is why the same steel appears more than once in the table.
- Cold-worked conditions are given in quarters of hard, from quarter hard to full hard. Tensile and yield strength rise with the amount of cold work and elongation falls.
- Hardness is given as a maximum for the soft conditions and is often not specified for the cold-worked ones, where the strength minimums already control the condition.
Table notes
Two values in the source table look like printing defects and are reproduced as printed rather than corrected. Type 205 in bar, plate, sheet and strip is given a hardness of 10 max HRB, where the annealed condition of every sibling type sits at 90 HRB or above. Type 202 cold-worked sheet and strip cite ASTM A 660 where every neighbouring row cites A 666. Types 347 and 348 in the hot finished and annealed condition carry no hardness value in the source table, and that cell is left blank here rather than filled in. The UNS numbers of types 321 and 321H are printed as S32100, 32109 in the source and are given here as S32100, S32109.
The values above are minimum acceptance values, not typical properties. A heat is tested against the minimum for its product form, so a certificate showing 620 MPa tensile on a type with a 515 MPa minimum is normal and not a different grade.
Composition data is for general reference only. Actual values vary by standard, mill, and heat number. Confirm against the material test certificate (MTC) or contact Aobo Steel. The martensitic stainless properties chart covers the 410, 420 and 440 series in the same way.
Austenitic against martensitic
The 300 series cannot be hardened by heat treatment and these minimums are reached by annealing or by cold work. The martensitic grades are hardened by quenching and tempering instead.
Yield is quoted at 0.2% offset
Austenitic stainless has no sharp yield point, so the standard uses the stress that produces 0.2 % permanent strain. Two suppliers quoting yield without saying which offset are not quoting the same number.
Cold work instead of alloy
Quarter hard 301 reaches about twice the yield strength of annealed 301 with no change in chemistry. That is the cheapest strength increase available in the 300 series and the reason spring and strip grades are ordered cold worked.
Related reference pages
Stainless steel composition chart · Martensitic stainless properties chart · Stainless steel physical properties chart · 420 stainless steel · 440C stainless steel · 4Cr13 stainless steel · Stainless steels overview
Source: ASM Handbook, Vol 1 (10th ed.), “Wrought Stainless Steels”, Table 7. Values are minimum room-temperature properties by product form and condition.
Austenitic stainless mechanical properties, printable PDF
Three A4 pages with the minimum tensile and yield strengths, elongation, reduction of area and hardness for 147 type, form and condition rows, the ASTM specification named in each row, and our contact details.