Martensitic Stainless Steel Properties Chart

Minimum mechanical properties of the standard martensitic stainless steels — 403 through 440C, including the free-machining and specialty types. Rows are grouped by type; each row gives a product form and condition with its tensile strength, yield strength, elongation, hardness and governing ASTM specification.

MPa / ksi same value, two units

(a)–(d) footnotes

(c) typical values

— not specified

FormConditionTensile
MPa
ksi0.2% yield
MPa
ksiElongation
%
Reduction
%
HardnessASTM spec
Type 403 (UNS S40300)
B, FAnnealed, hot finished48570275402045—A 276, A 473, A 479
BAnnealed, cold finished48570275401645—A 276
BIntermediate temper, hot finished690100550801545—A 276
BIntermediate temper, cold finished690100550801240—A 276
BHard temper, hot or cold finished825120620901240—A 276
WAnnealed48570275402045—A 580
WAnnealed, cold finished48570275401645—A 580
WIntermediate temper, cold finished690100550801240—A 580
WHard temper, cold finished825120620901240—A 580
P, Sh, StAnnealed485702053025 (b)—88 HRB maxA 176
Type 410 (UNS S41000)
B, FAnnealed, hot finished48570275402045—A 276, A 473, A 479
BAnnealed, cold finished48570275401645—A 276
BIntermediate temper, hot finished690100550801545—A 276
BIntermediate temper, cold finished690100550801240—A 276
BHard temper, hot or cold finished825120620901240—A 276
WAnnealed48570275402045—A 580
WAnnealed, cold finished48570275401645—A 580
WIntermediate temper, cold finished690100550801240—A 580
WHard temper, cold finished825120620901240—A 580
P, Sh, StAnnealed450652053022 (b)—95 HRB maxA 176
P, Sh, StAnnealed450652053020—95 HRB maxA 240
Type 410S (UNS S41008)
FAnnealed45065240352245—A 473
P, Sh, StAnnealed415602053022 (b)—88 HRB maxA 176, A 240
Type 410Cb (UNS S41040)
BAnnealed, hot finished48570275401345—A 276, A 479
BAnnealed, cold finished48570275401235—A 276, A 479
BIntermediate temper, hot finished8601256901001345—A 276, 479
BIntermediate temper, cold finished8601256901001235—A 276, A 479
E-4 (UNS S41050)
P, Sh, StAnnealed415602053022—88 HRB maxA 276, A 240
Type 414 (UNS S41400)
BIntermediate temper, cold or hot finished795115620901545—A 276, A 479
WAnnealed, cold finished1030 max150 max—————A 580
CA6NM (UNS S41500)
P, Sh, StTempered7951156209015—32 HRC maxA 176, A 240
B, FTempered795115620901545—A 276, A 473, A 479
Types 416 (UNS S41600) and 416Se (UNS S41623)
FAnnealed48570275402045—A 473
WAnnealed585-86085-125—————A 581
WIntermediate temper795-1000115-145—————A 581
WHard temper965-1210140-175—————A 581
Type 416 plus X (UNS S41610)
WAnnealed585-86085-125—————A 581
WIntermediate temper795-1000115-145—————A 581
WHard temper965-1210140-175—————A 581
Type 418 (UNS S41800)
B, FTempered at 620 °C (1150 °F)9651407601101545—A 565
Type 420 (UNS S42000)
BTempered at 204 °C (400 °F)17202501480 (c)215 (c)8 (c)25 (c)52 HRC (c)—
WAnnealed, cold finished860 max125 max—————A 580
P, Sh, StAnnealed690100——15—96 HRB maxA 176
TrimRite (UNS S42010)
WAnnealed690 max100 max—————A 493
WLightly drafted725 max105 max—————A 493
Type 422 (UNS S42200)
B, FTempered at 675 °C (1250 °F)8251205858517 (d)35—A 565
B, FTempered at 620 °C (1150 °F)9651407601101330—A 565
Lapelloy (UNS S42300)
B, FTempered at 620 °C (1150 °F)965140760110820—A 565
Type 431 (UNS S43100)
FIntermediate temper7951156209015——A 473
FHard temper121017593013513——A 473
WAnnealed, cold finished965 max140 max—————A 580
WAnnealed760110—————A 493
WLightly drafted795115—————A 493
Type 440A (UNS S44002)
BAnnealed725 (c)105 (c)415 (c)60 (c)20 (c)—95 HRB (c)—
BTempered at 315 °C (600 °F)1790 (c)260 (c)1650 (c)240 (c)5 (c)20 (c)51 HRC (c)—
WAnnealed, cold finished965 max140 max—————A 580
Type 440B (UNS S44003)
BAnnealed740 (c)107 (c)425 (c)62 (c)18 (c)—96 HRB (c)—
BTempered at 315 °C (600 °F)1930 (c)280 (c)1860 (c)270 (c)3 (c)15 (c)55 HRC (c)—
WAnnealed, cold finished965 max140 max—————A 580
Type 440C (UNS S44004)
BAnnealed760 (c)110 (c)450 (c)65 (c)14 (c)—97 HRB (c)—
BTempered at 315 °C (600 °F)1970 (c)285 (c)1900 (c)275 (c)2 (c)10 (c)57 HRC (c)—
WAnnealed, cold finished965 max140 max—————A 580
  • (a) B, bar; F, forgings; P, plate; Sh, sheet; St, strip; W, wire.
  • (b) 20% elongation for 1.3 mm (0.050 in.) and under in thickness.
  • (c) Typical values.
  • (d) Minimum elongation of 15% for forgings.

Table notes

Minimum mechanical properties for the standard martensitic stainless types, grouped by type — each row pairs a product form and condition with the properties guaranteed or typically expected in that condition. MPa and ksi columns are the same value in two units.

Hardness is given as Rockwell B, Rockwell C or Brinell exactly as printed (c) values are typical rather than guaranteed minimums. The spec column lists the ASTM specification each row is drawn from (A 276, A 473, A 479, A 580, A 581 and others).

In the source, one specification cell reads “A 276, 479”; it is read here as A 276, A 479.

Reference data for comparison — confirm the applicable specification and finish condition on the mill certificate before ordering or designing.

Related reference pages

420 stainless steel · 440C stainless steel · 440C stainless steel properties · 4Cr13 stainless steel · Stainless steel composition chart · 420 heat treatment · 440C heat treatment · 9Cr18Mo stainless steel · Stainless steels overview · D2 steel vs 440C · Stainless steel physical properties chart

Source: ASM Handbook, Volume 1 — Properties and Selection: Irons, Steels, and High-Performance Alloys, Table 11 “Minimum mechanical properties of martensitic stainless steels” (10th ed.). Reference data for comparison — verify the applicable standard before ordering.