Surface Roughness Chart

The Ra finish each production method leaves on steel, from flame cutting and sawing down to lapping and superfinishing. Each row shows the range routinely produced and the wider range that can still occur, in micrometers and microinches, along with the roughness grade numbers and their cut-off values.

Roughness produced by common production methods

The dark bar is the range a shop normally holds with that process. The grey bar shows the wider range possible under favorable conditions. Values as printed in Machinery’s Handbook 28th Edition, Table 1.

50 (2000) 2000 25 (1000) 1000 12.5 (500) 500 6.3 (250) 250 3.2 (125) 125 1.6 (63) 63 0.80 (32) 32 0.40 (16) 16 0.20 (8) 8 0.10 (4) 4 0.05 (2) 2 0.025 (1) 1 0.012 (0.5) 0.5 Ra, micrometres (microinches in brackets) Ra, microinches (bottom scale) Flame Cutting Snagging Sawing Planing, Shaping Drilling Chemical Milling Elect. Discharge Mach. Milling Broaching Reaming Electron Beam Laser Electro-Chemical Boring, Turning Barrel Finishing Electrolytic Grinding Roller Burnishing Grinding Honing Electro-Polish Polishing Lapping Superfinishing Sand Casting Hot Rolling Forging Perm. Mold Casting Investment Casting Extruding Cold Rolling, Drawing Die Casting average application less frequent application

Roughness ranges by production method, redrawn from the source chart. Left to right runs from rough to smooth.

ProcessAverage application, RaLess frequent application, Ra
Flame Cutting25 to 12.5 µm
1000 to 500 µin
50 to 6.3 µm
2000 to 250 µin
Snagging25 to 6.3 µm
1000 to 250 µin
50 to 3.2 µm
2000 to 125 µin
Sawing25 to 1.6 µm
1000 to 63 µin
50 to 0.80 µm
2000 to 32 µin
Planing, Shaping12.5 to 1.6 µm
500 to 63 µin
25 to 0.40 µm
1000 to 16 µin
Drilling6.3 to 1.6 µm
250 to 63 µin
12.5 to 0.80 µm
500 to 32 µin
Chemical Milling6.3 to 1.6 µm
250 to 63 µin
12.5 to 0.80 µm
500 to 32 µin
Elect. Discharge Mach.4.5 to 1.6 µm
180 to 63 µin
12.5 to 0.80 µm
500 to 32 µin
Milling6.3 to 0.80 µm
250 to 32 µin
25 to 0.141 µm
1000 to 5.66 µin
Broaching3.2 to 0.80 µm
125 to 32 µin
6.3 to 0.40 µm
250 to 16 µin
Reaming3.2 to 0.80 µm
125 to 32 µin
6.3 to 0.40 µm
250 to 16 µin
Electron Beam6.3 to 0.80 µm
250 to 32 µin
6.3 to 0.20 µm
250 to 8 µin
Laser6.3 to 0.80 µm
250 to 32 µin
6.3 to 0.20 µm
250 to 8 µin
Electro-Chemical3.2 to 0.20 µm
125 to 8 µin
12.5 to 0.05 µm
500 to 2 µin
Boring, Turning6.3 to 0.40 µm
250 to 16 µin
25 to 0.025 µm
1000 to 1 µin
Barrel Finishing0.80 to 0.20 µm
32 to 8 µin
3.2 to 0.05 µm
125 to 2 µin
Electrolytic Grinding0.566 to 0.20 µm
22.6 to 8 µin
0.80 to 0.10 µm
32 to 4 µin
Roller Burnishing0.40 to 0.20 µm
16 to 8 µin
0.80 to 0.10 µm
32 to 4 µin
Grinding1.6 to 0.10 µm
63 to 4 µin
6.3 to 0.025 µm
250 to 1 µin
Honing0.80 to 0.10 µm
32 to 4 µin
1.6 to 0.025 µm
63 to 1 µin
Electro-Polish0.80 to 0.10 µm
32 to 4 µin
1.6 to 0.012 µm
63 to 0.5 µin
Polishing0.40 to 0.10 µm
16 to 4 µin
0.80 to 0.012 µm
32 to 0.5 µin
Lapping0.40 to 0.05 µm
16 to 2 µin
0.80 to 0.012 µm
32 to 0.5 µin
Superfinishing0.20 to 0.025 µm
8 to 1 µin
0.80 to 0.012 µm
32 to 0.5 µin
Sand Casting25 to 12.5 µm
1000 to 500 µin
50 to 6.3 µm
2000 to 250 µin
Hot Rolling25 to 12.5 µm
1000 to 500 µin
50 to 6.3 µm
2000 to 250 µin
Forging12.5 to 3.2 µm
500 to 125 µin
25 to 1.6 µm
1000 to 63 µin
Perm. Mold Casting3.2 to 1.6 µm
125 to 63 µin
6.3 to 0.80 µm
250 to 32 µin
Investment Casting3.2 to 1.6 µm
125 to 63 µin
6.3 to 0.40 µm
250 to 16 µin
Extruding3.2 to 0.80 µm
125 to 32 µin
12.5 to 0.40 µm
500 to 16 µin
Cold Rolling, Drawing3.2 to 0.80 µm
125 to 32 µin
6.3 to 0.20 µm
250 to 8 µin
Die Casting1.6 to 0.80 µm
63 to 32 µin
3.2 to 0.40 µm
125 to 16 µin

Roughness grades N1 to N12

Older drawings and specifications call out the grade number instead of an Ra value. The grade numbers run the other way round to Ra, the higher the number the rougher the surface. Source, Table 4.

GradeRa, µmRa, µin
N12502000
N11251000
N1012.5500
N96.3250
N83.2125
N71.663
N60.8032
N50.4016
N40.208
N30.104
N20.052
N10.0251

Preferred Ra values to specify

The standard series of Ra values (ISO 1302 and the equivalent national standards). The values marked (a) are the recommended ones, and specifying a value from this series keeps the part measurable with standard roughness specimens. Source, Table 3.

Preferred series of Ra values, µm (top) and µin (bottom)
0.012
0.5
0.025 (a)
1
0.050 (a)
2
0.075
3
0.10 (a)
4
0.125
5
0.15
6
0.20 (a)
8
0.25
10
0.32
13
0.40 (a)
16
0.50
20
0.63
25
0.80 (a)
32
1.00
40
1.25
50
1.60 (a)
63
2.0
80
2.5
100
3.2 (a)
125
4.0
160
5.0
200
6.3 (a)
250
8.0
320
10.0
400
12.5 (a)
500
15
600
20
800
25 (a)
1000

(a) Recommended values.

Cutoff, the roughness sampling length

The cutoff is the length over which the instrument samples the profile. Where the drawing does not state one, the 0.80 mm (0.030 in.) value applies. Source, Table 2.

Cutoff, mmCutoff, in.
0.080.003
0.250.010
0.800.030
2.50.1
8.00.3
25.01.0
  • Ra is quoted in micrometres and microinches throughout, the two rows of the source chart.
  • A surface machined by one process is often improved by a later finishing process in the chain, turned, then ground, then honed. Read the chart left to right for the processes that follow.
  • The ranges are general shop values. The finish a cut actually leaves depends on the material, the tool or wheel, the rigidity of the setup and the feed used.

Reading the chart

The process rows run from the roughest finishes at the top to the smoothest at the bottom, and the scale runs from Ra 50 µm on the left to 0.012 µm on the right. A grey bar that extends past a value means the process can reach that roughness under favourable conditions, and the dark section is where the process usually sits. When a drawing calls for a finish, check that the process named for the part’s last operation can hold it. A milled surface is usually quoted at Ra 3.2 to 0.80 µm, so grinding or lapping follows when the drawing is tighter.

How fast the steel can be machined, and with which tool, is covered in the machinability rating chart and in the cutting speeds and feeds for tool steels. Surface treatments that add a layer rather than cut one are a different subject, on the surface treatment page.

Machining allowance chart · Tool steel properties chart

Source: Machinery’s Handbook 28th Edition (Industrial Press), Surface Texture section: Table 1 (roughness produced by common production methods), Table 2 (standard cutoff values), Table 3 (preferred series of Ra values), Table 4 (roughness grades). The chart is redrawn from the source. Values are converted between micrometres and microinches at 1 µm = 39.37 µin (0.0254 µm = 1 µin).