Nitriding of Tool Steels

Nitriding adds a hard, wear-resistant case to a finished tool without quenching, so the part keeps its size and core toughness. This page collects what the treatment produces on tool steels, the depth and hardness it is normally held to, the layer structure behind the surface, and the places in die and mold work where it earns its cost.

What nitriding produces on a tool steel

The values below are the working range for H-series and comparable tool steels. A deeper case isn’t better in tooling because the same nitrogen that raises hardness also raises the layer’s brittleness.

ItemValueWhat it means in practice
Typical values for tool steels
Nitriding depth0.1–0.2 mmThe hardened case that carries the wear. Depths of 0.5–1.0 mm indicate carburizing and are a common mistake when copying targets from that process.
Surface hardness1000–1200 HV0.5Typically reached on H-series tool steels in gas nitriding. Above 1000 HV is easy for these grades, and the hardness depends on how much chromium and aluminium the steel carries.
Process temperature525–545°CBelow the tempering range of most tool steels, so the part is nitride after the final hardening and tempering rather than before it.
Process time4–10 hThe usual range in practice. Longer treatments deepen the case and thicken the compound layer rather than raising the surface hardness.
Core hardnessUnchangedThe interior keeps the hardness and toughness of the tempered part, which is why the treatment suits finished tooling.
Hardening mechanismAlloy nitridesNitrogen diffuses in and precipitates fine alloy nitrides, chromium being the main former in tool steels, aluminium the strongest one where a grade is built with it.

Source: Tool Steels, Properties and Performance (R. A. Mesquita, CRC Press), Section 4.2.3 and the measured response curves in Figure 4.11.

The surface layer and the hardened zone

Nitrogen concentration at the surface decides which layer forms. The same equipment runs all three ranges by changing the atmosphere, so the layer is a process choice rather than a property of the steel.

Layer formedAtmosphereStructureWhere it is used
Diffusion layer only1–5% N2None. The hardened zone is a gradient of precipitated nitrides in the steel.Crack-sensitive tooling such as die-casting dies, where a brittle skin is not acceptable.
Compound layer, γ′ type15–30% N2Fe4N on top of the diffusion layerWear surfaces that can carry a hard skin. The layer is harder than the matrix but less brittle than the ε type.
Compound layer, ε type60–70% N2 with 1–3% methaneFe2-3N on top of the diffusion layerMaximum surface hardness, with the highest brittleness. Usually avoided on parts that see cracking or impact.

Source: Tool Steels, Properties and Performance (R. A. Mesquita, CRC Press), Figure 4.12, adapted there from the ASM Handbook on heat treating. The compound layer is called the white layer in the shop because it stays bright under the microscope and resists the usual etch.

The two layers do not appear at once, and the order in which they form determines which one the finishing operation must deal with.

Formation of the compound zone: nitrogen from the atmosphere building the epsilon and gamma-prime nitride layers at the steel surface
Fig. 8.9. Formation of the compound zone. Nitrogen from the atmosphere first forms gamma-prime nitride at the steel surface, and the epsilon nitride layer grows over it as the nitrogen supply continues. The example is a plain nitriding steel; the layer sequence is the same on the chromium-bearing tool steels, where the same cycle produces a thinner layer. Source: D. Pye, Nitriding Techniques, Ferritic Nitrocarburizing, and Austenitic Nitrocarburizing Techniques and Methods, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 8.9.

Why the white layer gets a bad name

The compound layer is a ceramic skin on a steel part, and it is very hard and very brittle. Used well, it is the highest hardness the treatment can produce. Used poorly, it can cause cracks that end a die’s life. The source shows both outcomes on H13, first a diffusion layer alone, then a case where a thick white layer and carbonitride precipitates along the grain boundaries turned into crack paths, with the cracks travelling through the compound line rather than around it.

Two shop rules follow. On parts that see impact or thermal cycling, keep the layer thin or suppress it; for a nitrided forging die, the source sets the practical limit at 0.25 mm of layer, below which cracking stays rare. On parts that only slide, a controlled compound layer adds the most wear resistance for the least case depth.

What the measured case looks like

In the response curves published with the data, gas nitriding at 530°C for 36 hours brings an H11 modified steel to about 1200 HV0.5 at the surface, holds close to that value through the first 0.1 mm, and then falls back to the 600 to 650 HV0.5 of the tempered core by roughly 0.3 mm. A shorter cycle of 525°C followed by 545°C for 10 hours reaches a similar surface level of about 1100 to 1200 HV0.5 on H13, H11, and a modified H10, again returning to the core hardness within roughly 0.3 mm.

Source: Tool Steels, Properties and Performance (R. A. Mesquita, CRC Press), Figure 4.11, gas nitriding response curves for H11 modified (X38CrMoV5-1), H13 (X40CrMoV5-1) and a modified H10 (X50CrMoV5-3). Values are read from the published curves at the surface and at depth.

Reading the curves

The case depth in the hardness profile and the nominal nitriding depth quoted in the literature are measured differently. The profile above describes a long cycle at 36 hours, and its useful hardened depth runs beyond the 0.1 to 0.2 mm the source quotes as the typical tool-steel target. Whichever number you quote, measure the case on the part or on a coupon that saw the same cycle, because furnace load, gas flow and surface condition all shift the result.

Published hardness profiles for four nitriding steels show the shape the cycle above produces.

Hardness gradients of gas nitrided 41CrS4, 31CrMoV9, 15CrMoV59 and 40CrMoV51 tool and nitriding steels, hardness HV0.5 against distance from the surface
Fig. 7.50. Hardness gradients of nitrided steels: 41CrS4, 31CrMoV9, 15CrMoV59 and the hot work grade 40CrMoV51 (1.2344, directly comparable with H13), plotted as HV0.5 against distance from the surface. The hardest material sits in the first tenths of a millimeter, and the profile falls back to the tempered core hardness further in, which is the case depth that matters in service rather than the nominal nitriding depth. Source: J. Grosch, Heat Treatment with Gaseous Atmospheres, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 7.50.

Gas, plasma and salt

Gas nitriding feeds nitrogen from a dissociated ammonia atmosphere and is the process the published data for tool steels mostly comes from. Plasma nitriding strikes nitrogen in an ionized gas instead, giving finer control over the layer and letting the shop shield areas that should stay soft. Liquid salt bath nitriding is fading for environmental reasons. The layer structure behind the three is the same, so the choice comes down to equipment, control, and cost rather than a different result.

Nitride after hardening and tempering, never before

The treatment runs at a lower temperature than the tempering step, so it cannot harden the steel itself. It is applied to a part that is already at its final hardness, which is also why the part keeps its size through the process. A part that goes to the nitriding furnace with a soft core comes back with a hard skin on a soft core, and the first loaded contact finds out.

Nitriding is not carburizing

Carburizing runs near 900 to 1000°C, diffuses carbon for a fast and deep case, and depends on a quench afterward to harden the surface by martensite. Its ceiling is martensite hardness, around 900 HV, and the case can soften again during later tempering. Nitriding runs near 540°C on the finished part, hardens by nitride precipitation rather than by a quench, and passes 1000 HV without a second heat treatment. Case depth targets do not transfer between the two processes.

Aluminium in the grade answers the nitriding furnace

The hardness of a nitrided case comes from whichever alloying elements form the nitrides, and aluminum forms the strongest ones. Grades that carry aluminum as a deliberate addition, such as some extrusion and precipitation hardening mold steels, reach a much harder case than a plain 5% Cr hot work steel under the same cycle. When a drawing specifies a nitrided hardness above the usual range for H13 or H11, the grade itself is usually the lever, not the furnace.

The nitriding potential and temperature determine which nitride forms in the compound layer, and the Lehrer diagram maps it.

Lehrer diagram: nitriding potential against temperature, with the alpha, gamma-prime and epsilon nitride stability fields
Fig. 7.56. The Lehrer diagram: nitriding potential against temperature. Above the upper curve the compound layer is epsilon nitride, between the two curves it is gamma-prime, and below the lower curve no compound layer forms at all and the case is a diffusion zone only. This is the standard map for setting a gas nitriding atmosphere; the boundaries shift slightly with alloy content, which is why you read the diagram alongside a test coupon. Source: J. Grosch, Heat Treatment with Gaseous Atmospheres, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 7.56.

The iron-nitrogen system behind those layers is narrow, which is why nitriding is run at that temperature.

Iron-nitrogen equilibrium diagram showing the alpha, gamma-prime, epsilon and gamma phase fields and the 590 C eutectoid
Fig. 8.18. Iron-nitrogen equilibrium diagram, with the alpha, gamma-prime, epsilon and gamma fields marked. The solubility of nitrogen in ferrite is a fraction of a percent and falls to almost nothing at room temperature, and the eutectoid in this system sits at 590 °C. That ceiling is the reason the practical nitriding range stops at about 570 °C: above it the treatment is no longer a ferritic diffusion process. Source: D. Pye, Nitriding Techniques, Ferritic Nitrocarburizing, and Austenitic Nitrocarburizing Techniques and Methods, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 8.18.

Plasma nitriding does the same job through a glow discharge rather than ammonia alone.

The ion nitriding mechanism: cathode fall, plasma, glow border, ion and electron reactions and the epsilon and gamma-prime phases formed in the surface
Fig. 8.19. The ion nitriding mechanism. Nitrogen and hydrogen ions are accelerated across the cathode fall and strike the workpiece, giving up nitrogen that diffuses into the surface; iron sputtered from the workpiece recombines with nitrogen in the plasma and returns to it. The epsilon and gamma-prime phases form in the same sequence as in gas nitriding. The figure is credited in the source to the ASM Handbook, Volume 4. Source: D. Pye, Nitriding Techniques, Ferritic Nitrocarburizing, and Austenitic Nitrocarburizing Techniques and Methods, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 8.19.

Where it pays for itself

Hot forging is where nitriding is applied most, because the die surface sees load and abrasion above 500°C and the surface hardness is the deciding factor. Hot extrusion follows, and the aluminium treated grades above were developed for it, along with the ESR H13 used in extrusion work. Die casting is the careful case, because the thermal cycling cracks a brittle layer quickly, so the compound layer is kept thin. In plastic molds the treatment is the normal way to protect a hardened plastic mold steel cavity against wear and to hold the polished finish, and it is one of the reasons an ESR refined H13 above 50 HRC is popular for lenses and other work that leaves the mold bright. The polishing and texturing side of that work, including the defects a nitrided surface changes, is covered in the mold steel polishing and texturing guide.

The heat treatment sequence around the furnace is in the hardening and tempering chart, and how a nitrided case behaves at temperature alongside the base hardness of the grade is in the hot hardness chart. The other surface treatments that compete with it, including PVD coating and hard chrome, are compared in the surface treatment guide.

Confirm before quoting

Case depth, hardness and layer structure are for general reference only. Actual results vary by grade, furnace, gas mixture and part geometry. Confirm the process with your heat treater and the grade data with the mill before production. Aobo Steel supplies tool steel in the annealed or prehardened condition, and nitriding remains a service performed on the finished tool.

Tool steel heat treatment guide · Tool steel processing characteristics · Selection of tool steel for hot extrusion dies · Selection of tool steel for die casting cores and inserts · Hot work tool steels · Why H13 is used in die casting · Ion implantation for tool steel dies