Steel Grades and Compositions for Pattern-Welded Blades

Compositions in weight percent for the eleven steel grades that the source lists for pattern-welded blades, split into the dark and the bright series that a smith pairs for contrast, plus the two powder metallurgy grades used for pre-damasked billets. Fe is the balance of every row and the values are printed as they appear in the source table. This page is a reference summary of published practice and not an Aobo Steel specification.

Composition of the dark series grades

The dark series etches dark in acid and carries most of the carbon of the billet.

GradeC
%
Si
%
Mn
%
P
%
S
%
Cr
%
Ni
%
Mo
%
V
%
Cu
%
10840.80—0.600.0400.050—————
10950.9–1.03—0.3–0.50.0400.050—————
51600.560–0.6400.150–0.30.75–10.0350.040.7–0.9————
521000.98–1.100.15–0.300.25–0.450.0250.041.30–1.60————
20C1.000.300.450.0150.00050.15————
90MCV80.8—2——0.4——0.10—
W-20.6–1.40———————0.25—

Source, Damascus and pattern-welded steels, Forging blades since the iron age (M. Durand-Charre), Table 7.3.1, p. 99. Composition in weight percent, Fe balance, arranged one element per column.

Composition of the bright series grades

The bright series etches light. The contrast comes from nickel, 2 % in 15N20 and 3.25 to 4.3 % in the two nickel steels.

GradeC
%
Si
%
Mn
%
P
%
S
%
Cr
%
Ni
%
Mo
%
V
%
Cu
%
L60.70.5————1.750.50.250.25
15N200.750.300.400.0180.0050.112———
45NCD160.40.50.2–0.50.030.031.23.8–4.30.15–0.35——
ASTM 203 E0.230.15–0.300.80.0350.04—3.25–3.75———

Source, Damascus and pattern-welded steels, Forging blades since the iron age (M. Durand-Charre), Table 7.3.1, p. 99. Composition in weight percent, Fe balance, arranged one element per column.

Powder metallurgy grades for damascus billets

Pre-damasked bars are sintered from two atomised powders instead of forge welded from plate. RWL 34 is the harder steel of the pair and finishes bright after etching, PMC 27 is softer and finishes dark. The two together reach about 60 HRC, and the producer reports the beginning of fusion at 1220 °C, so the forging temperature has to be held well below that point. Damasteel is a trade mark of its owner.

GradeC
%
Si
%
Mn
%
P
%
S
%
Cr
%
Ni
%
Mo
%
V
%
Cu
%
RWL 341.050.50.5——14—40.2—
PMC 270.60.50.5——13.5————

Source, same book, section 7.5 Sintered steels, p. 111. Composition in weight percent as printed for the two grades of the Damasteel process.

Pattern-Welded Blade Steel Compositions, printable PDF

One A4 page with the eleven dark and bright series grades and the two powder metallurgy grades in weight percent, the pair selection notes and our contact details.

The two carbon grades in the dark series are covered in more detail on the carbon steel composition chart, the bearing grade on the 52100 steel properties page and the bright grade L6 on the L6 tool steel page. For the knife side of the same subject see knife steel types.

A pair is chosen for four things. The two grades have to sit at opposite ends of the etch response, one dark and one bright, or the pattern disappears. Their melting points have to be close enough for the layers to weld, and their thermal expansion has to match, because layers that move differently can break the weld when the blade cools. Manganese in the stack stops graphite forming when a forging session runs long, and chromium slows the diffusion of carbon between the layers so the layers stay distinct instead of homogenising into one steel. Nickel does not form carbides and pushes carbon towards graphite, which is why the nickel bearing layers in the table also carry manganese.

A common construction is a hard core wrapped in a pattern welded skin. The core is chosen for edge holding, the skin for the pattern and for toughness at the spine. Pure nickel and pure iron are also used in the stack for a bright line, but both are soft and are not used for the cutting layer.

The figures above are the values printed in the source table. They differ from current mill specifications for some of the same designations, so confirm chemistry, hardenability and heat treatment against the applicable standard and the material test certificate before ordering. Aobo Steel supplies tool steel in bar and plate form and does not produce pattern welded billets.

Reference data compiled from Damascus and pattern-welded steels, Forging blades since the iron age (Madeleine Durand-Charre), table 7.3.1 and section 7.5.