Sorting Steel Bars Without Cutting Them
A mixed lot of bar, or a single bar that will not reach the hardness the order calls for, is expensive to discover after the die is cut. The alternative to a cut, a hardness test and a chemical check is an electromagnetic pass down the bar, and it can report a change of grade, a change of hardness and a seam in the same trip. This page sets out what that pass can and cannot separate, and the coil set and gate positions that make it work.
Two families of electromagnetic test
An electromagnetic system reads how a bar loads a coil carrying alternating current, and the reading changes with both the electrical conductivity and the magnetic permeability of the steel. A system built on conductivity is called an eddy current system, and a system built on permeability is called a magnetic permeability system. Both detect flaws in a bar, and their reach is very different.
On a ferromagnetic bar, the magnetic effect is so much larger than the eddy current effect that it hides it, and the standard remedy is to magnetically saturate the bar with a direct current solenoid or a strong permanent magnet so that only the conductivity effect is left. When the permeability effect is deliberately used instead of suppressed, the test is more properly called an electromagnetic or magnetoinductive method. One useful consequence follows from this. Above the Curie temperature the steel is no longer magnetic, so a hot bar can be inspected by eddy current without saturation, and for the same reason a permeability system cannot be used on a hot bar at all.
How far eddy current reaches into the bar
Eddy currents concentrate near the surface of the part nearest the coil, and the concentration grows as the frequency rises, so the operating frequency sets the depth the test can see. A typical system varies its frequency in discrete steps from 0.5 kHz to 1000 kHz, and the range most used for general flaw detection is 1 to 50 kHz. Dedicated packages vary the frequency, the phase and the filters together, and the aim is always to get the best signal to noise on the flaw of interest without wasting sensitivity on a depth the bar does not need to be checked at.
On steel bar the method is particularly good on seams. Depending on the circuit used, a difference of as little as 0.025 mm, or 0.001 in., in seam depth can be detected by an eddy current system. That figure is the reason eddy current became the production method for drawn bar and wire, where a tight longitudinal seam is the flaw that matters most.
Where the property being sorted is conductivity itself, the useful spread is large between a pure metal and a high-alloy one, and the published table makes the point. Conductivity is quoted against the International Annealed Copper Standard, in which unalloyed annealed copper is 100 percent, and it is measured from the resistivity of the material.
| Metal or alloy | Resistivity, microhm mm | Conductivity, % IACS |
|---|---|---|
| Silver | 16.3 | 105 |
| Copper, annealed | 17.2 | 100 |
| Gold | 24.4 | 70 |
| Aluminum | 28.2 | 61 |
| Aluminum alloy 6061-T6 | 41 | 42 |
| Aluminum alloy 7075-T6 | 53 | 32 |
| Aluminum alloy 2024-T4 | 52 | 30 |
| Magnesium | 46 | 37 |
| 70-30 brass | 62 | 28 |
| Phosphor bronzes | 160 | 11 |
| Monel | 482 | 3.6 |
| Zirconium | 500 | 3.4 |
| Titanium | 548 | 3.1 |
| Zircaloy-2 | 720 | 2.4 |
| Type 304 stainless steel | 700 | 2.5 |
| Inconel 600 | 980 | 1.7 |
| Hastelloy X | 1150 | 1.5 |
| Waspaloy | 1230 | 1.4 |
Electrical resistivity and conductivity of common metals and alloys, reproduced from Table 1 of Eddy Current Inspection in ASM Handbook, Volume 17. The table is set on nonferrous metals because those are the ones sorted by conductivity, and it shows that conductivity also shifts with temperature, composition, heat treatment and residual stress, which is what allows a conductivity sort to track heat treatment and hardness in an alloy where those changes move the reading enough.
The coil set that reports three things in one pass
The systems that sort bar use a primary coil wound on the bar, two null coils and two standard coils, with all three circuits independent so that a single pass down the bar gives three readings at once. The null circuit is the flaw detector. Its two matched coils are connected in opposition, and the section of bar between them sets the meter to zero, so a flaw in that window shows up as a deflection. The coils are spaced 75 to 102 mm apart because a normal seam tapers into sound material over about 75 mm of length, and the run that has to fit inside the window is what makes the reading reliable.
The two standard circuits do the sorting. Each carries only one winding on the bar and balances it against an adjustable voltage in the instrument, so the reading is a comparison between the bar in the coil and the setup bar that was used to zero it. One standard circuit reports a different grade or a full-length seam or crack, and the other reports a change of hardness or structure. Because the circuits are independent, both are read at the same time as the flaw signal.
| Coil set in the test head | What it reports |
|---|---|
| Primary coil | Excites the bar at line frequency, adjustable from 1000 to 30,000 ampere turns and usually set between 10,000 and 15,000 |
| Two null coils | A matched pair spaced 75 to 102 mm apart and connected in opposition, so the meter reads a flaw in the section between them |
| Standard coil A | Compares every bar against the setup bar and reports a different grade or a full-length seam or crack |
| Standard coil B | Compares every bar against the setup bar and reports a change of hardness or structure |
The coil set used for the simultaneous detection of flaws and of variation in composition, structure and hardness in steel bars, reproduced from Nondestructive Inspection of Steel Bar, Wire and Billets in ASM Handbook, Volume 17. The whole assembly is set on the bar in a single pass.
Reading a mixed lot
A reading on a standard circuit has to be interpreted against its length. If the meters run off for the whole length of the bar, the bar is likely a different grade or it carries a full-length seam or crack. If the reading varies along the bar, the cause is more likely a change of hardness or structure, or it is a deep flaw, and a deep flaw will show on the null circuit at the same time. The two readings together are what separate a grade mix-up from a hardness variation.
Two rules keep the sort honest. The bar used to set the instrument is set aside until the whole lot has been tested, because every other bar is being compared against it, and a setup bar that is itself off grade hides the very mix-up the test is looking for. And when a group of unwanted bars has been separated out, it pays to retest that group with one of its own bars as the setup, because a mixed lot of steel often contains a third grade as well as the one that was being removed.
Where the gates sit on the wave
The three readings come from three electronic gates placed at different points on the waveform, because hardness, grade and structure each shift the wave at a different place. The gates are normally placed 8 to 20 degrees either side of the stress peaks, where the effect of workload stress on the wave is smallest and a flaw changes the shape cleanly. A second gate can then be set to watch the part of the wave where a flaw changes the saturation level, if the material and size allow the test to reach saturation at all.
In the published procedure for one instrument the three gates are placed roughly as follows on a bar of 1141 steel, and the same separation is what any operator looks for on another grade.
| Gate position on the wave | What that gate is set to report |
|---|---|
| Near the low end of the half cycle, about 10 to 30 degrees | Hardness |
| Across the top of the half cycle, near 90 degrees | Grade |
| On the falling side of the top of the half cycle, about 90 to 120 degrees | Structure |
The three electronic gate positions used to inspect one lot of bar for hardness, grade and structure, reproduced from the sorting example and Fig. 21 of Nondestructive Inspection of Steel Bar, Wire and Billets in ASM Handbook, Volume 17. The angles are read from an oscilloscope trace of one half of an electrical cycle, and every bar in the lot is compared against the setup bar.
What the method will not do
A permeability system needs a bar to carry a uniform level of residual stress, and a few stock conditions deny it that. Hot rolled or annealed bar cannot be sorted by permeability unless it has first been given some uniform cold work, such as a rotary straighten on round bar or a planar straighten on square, hexagonal or flat sections. Gag-straightened bar is unsuited to the method, because the ram leaves concentrations of stress far above the level left by a flaw elsewhere in the bar, and those concentrations swamp the reading. The condition ranking below is the source order.
| Stock condition | Flaw detection efficiency by the permeability system |
|---|---|
| Heat treated, quenched, drawn and machine straightened | Highest |
| Cold drawn and machine straightened | High |
| Cold drawn, annealed and machine straightened | Medium |
| Hot rolled and machine straightened, centerless ground | Low |
| Hot rolled and machine straightened | Lowest |
Efficiency of flaw detection by a magnetic permeability system against the condition of the bar, reproduced from Nondestructive Inspection of Steel Bar, Wire and Billets in ASM Handbook, Volume 17. After straightening, the bars should be aged for 24 to 48 hours near room temperature, or stress relieved at up to 260 C, for best sensitivity.
Sorting steel bars without cutting them, printable PDF
The two electromagnetic test families, the conductivity table, the coil set that reports three things at once, the three gate positions and the condition ranking, in one PDF with our contact details.
Grades and stock
Sorting answers a different question from the one a flaw detection report answers, and the two together cover a bar in one pass. What each flaw looks like when it turns up is described on the steel bar defects page, and the full set of checks behind a mill certificate is collected on the steel bar and billet inspection page.
Hardness is the property most often sorted for, and the bench and portable methods that confirm a sorted bar are set out on the hardness testing methods page. Where the concern is a grade mix-up rather than a hardness variation, the chemical side is on the page on how steel chemistry is tested, and the way the bar should arrive with its test report is on the bar delivery condition page.
A sort answers a question about a lot rather than about a single bar, and the flaw side of the same test on bar and billet is described on the bar and billet inspection page. What each nondestructive method needs from the material, and how thick and how complex a part each one can handle, is collected on the page on choosing a nondestructive test method.
Sorting steel bars without cutting them, printable PDF
The two electromagnetic test families, the conductivity table, the coil set that reports three things at once, the three gate positions and the condition ranking, in one PDF with our contact details.
Before you use these values
This page is a reference summary of published practice and it is not an Aobo Steel specification. The conductivity values, the coil set and the gate positions are reproduced from the source, and the settings that suit one grade on one instrument have to be established on that instrument before a lot is released. Final acceptance is set by the purchase specification.
Source: ASM Handbook, Volume 17, Nondestructive Evaluation and Quality Control, ASM International, 1989.