Ram Speed, Puller Speed and Acceleration: Where the Cycle Time Actually Goes

An extrusion press spends its day in two states: pushing metal and not pushing metal. The pushing part gets all the attention, but the seconds before the press reaches steady speed are paid for on every single billet, and they are longer on the dies with the lowest extrusion ratio — which are often the dies running the highest-value sections. This page is the arithmetic behind that: how ram speed and puller speed relate, what the acceleration ramp does to the cycle, and the three published levers for shortening it without pushing the exit temperature out of range.

Exit speed, ram speed, and the ratio in between

Without a puller, the speed of the metal leaving the die is the ram speed multiplied by the extrusion ratio:

VE = VR × ER, where ER is the container bore area divided by the total area of the extrusion, taking the number of holes in a multihole die into account.

That is the number a press operator can work out from the die print before the die is even loaded. It is also the number that decides whether a given ram speed is legal: the exit speed sets the temperature rise at the bearing, and the exit temperature sets the surface.

What the puller changes

A puller does not simply take the extrusion away; it stretches it while it is hot, which thins the section and therefore raises the speed for the same volume of metal. The published relationships are:

  • VP = VE + ΔVP — the actual puller speed is the free exit speed plus the increase caused by puller tension.
  • AE × VE = AP × VP — volume constancy between the die exit and the pulled section.
  • VP = VR × (ER)m — the puller speed equals ram speed times a modified ratio, where the modified ratio uses the final, pulled area instead of the die area.

The practical use of the third equation is a calibration check that costs nothing. Calculate the puller speed from ram speed and the modified ratio, then compare it with the puller speed on the electronic readout. If the two agree, the puller tension is doing what the setting says. If they do not, either the tension or the section is not what the paperwork claims — and both are worth knowing before the next billet rather than after the next complaint.

What a puller is for, beyond speed, is on the published list of advantages: less labour, less scrap, help in controlling metal flow through the die, and the ability to cut the extrusion into multiple lengths without stopping the press. The puller is closed-loop linked to the press cycle, so it stops when the press stops, and it carries the section through the air or water quench after the die. On a 6xxx line running a feeder plate die, that combination is what makes continuous extrusion possible.

The acceleration ramp, and why low ratios hurt

Measured on 6063, the extrusion speed at the start of a stroke does not jump to its steady value: it climbs slowly and then levels off. The published model treats the climbing part as a straight line with a slope, and the slope is a function of the process variables — which is what makes the ramp controllable rather than mysterious.

Two effects are worth remembering, because they point in opposite directions to what a press operator might expect.

Extrusion ratio. Higher ratio means higher steady speed, as the equation says. But the acceleration time also increases with the ratio, which means the slope of the acceleration curve decreases as the extrusion ratio decreases. A low-ratio die — a heavy, simple section — does not accelerate quickly; it spends a larger share of its stroke getting up to speed.

Billet temperature. The slope increases with billet temperature, so a hotter billet shortens the acceleration time. That is the cheapest lever on the list and the easiest to abuse, because raising the billet temperature also raises the exit temperature.

The limit on heating the billet to save time

There is a hard stop, and the published version of it is two checks rather than one number. Before accepting a higher billet temperature to cut acceleration time, confirm:

  • That the exit temperature still lands inside the solution temperature range the alloy needs for its properties after heat treatment.
  • That the exit temperature does not reach the hot shortness range of the alloy being extruded.

Those two conditions define the optimisable window. Any billet temperature that satisfies neither adds speed and subtracts quality, and the cost shows up not at the press but in the quench, the temper and the surface.

Three levers, in the order they should be tried

The published ways to shorten acceleration time are procedural and cheap, and they should be tried in this order because the first two do not touch the metal:

LeverWhat it doesWhat it costs
Increase ram speed at fixed billet temperatureShortens the ramp by starting from a higher speedExit temperature rises; check against the two limits above
Reduce the extrusion ratio by adding holes to the dieShortens acceleration time directly; also lowers pressureA new die, and the per-hole ratio has to stay workable
Adjust initial billet temperature at fixed ram speedSteepens the slope, so the press reaches steady state soonerEats into the exit temperature window

Published levers for reducing acceleration time. The fourth route in the source is not a press setting at all: improve the extrudability of the alloy by compositional adjustment or by an optimal homogenization practice.

That fourth route is the one that gets forgotten, because it belongs to the billet supplier rather than the press. Published work on billet preheating found a sharp increase in extrudability at high billet temperatures — 30% and 60% for two AlMgSi alloys — and a further gain from homogenizing and then cooling back into the normal temperature range before extrusion. The extrusions that ran fastest also had better mechanical properties and surface quality than those from billets heated directly into the normal preheating range. Extrudability is not a fixed property of an alloy; it is a property of the billet you were sold.

What this does to the shift, not just the billet

Cycle time is the sum of the press doing work and the press doing nothing, and the published productivity levers are stated in exactly those terms: minimise avoidable scrap per billet run, maximise billet length to use the press capacity and the runout table, and optimise speed while compensating for the temperature rise during the stroke. The acceleration ramp sits inside the third of those, and it is the one that is invisible on a shift report because nothing records the seconds before steady state.

The measurement that makes it visible is the billet push time, which is already a field on the published extrusion process checklist, together with the number of billets extruded and the runout calculated against runout actual. A die that needs two seconds longer to accelerate costs two seconds per billet — on a run of forty billets, that is most of a minute of press time for one die, and it repeats every order the die is used on.

Where this leaves a die steel order

Two of the levers in this page are die decisions, not press decisions: the number of holes, and therefore the extrusion ratio per hole, is fixed when the die is designed; and the ratio the die is designed for decides how long it takes to accelerate. A die shop that wants to be useful to a customer chasing cycle time should be able to say what the ratio per hole is, what the exit speed will be at the customer’s ram speed, and what that does to the bearing temperature.

The steel side of that conversation is the grade and its hot hardness on the H13 tool steel page, the ESR programme for extrusion tooling on the 1.2344 ESR H13 page, the land that sets the exit temperature on the die bearing length page, the multi-hole and feeder-plate options on the die types and tooling page, and the exit-temperature mechanism itself on the die temperature and isothermal extrusion page.

Before you change a speed from this page

The relationships here are published identities and the 6063 behaviour is from a published test series, not from your press. Ram speed, puller tension and billet temperature are set per die, per alloy and per press, and the only number that transfers is the check: exit temperature inside the solution window and below the hot shortness range. Measure the push time and the puller speed against the calculation before optimising anything.

Source, Aluminum Extrusion Technology, P. K. Saha, ASM International, 2000, chapter 6, ram and extrusion speed control and productivity control, pages 158 to 162 and 170 to 172.