Die Temperature and Isothermal Extrusion: What the Exit Reading Is Really Telling You
Billet temperature is what the furnace delivers. Exit temperature is what the metal is actually at when it leaves the bearing, a few centimetres and a few hundred degrees of deformation later, and it is the only one of the two that decides whether the surface survives and whether the section can still be quenched to temper. Heat comes from plastic work and from friction at three separate interfaces, and it goes into the extrudate, the container, the die and the unextruded part of the billet at the same time. This page sets out where that heat comes from, which variables move it, how it is measured in a plant, and what isothermal extrusion actually does about it.
The alloy-by-alloy temperature windows — solidus, homogenization soak, extrusion range — are on the extrusion temperature page. This page starts where that one stops: the exit side of the die and the control loop around it.
Where the heat comes from
Most of the work of deformation becomes heat, and the temperature rise from plastic deformation alone can reach several hundred degrees. Friction adds to it at three places: the billet against the container bore, the flowing metal against the dead-metal zone, and the metal against the die bearing. Some of that heat leaves in the extrudate, some conducts into the container and the die, and some goes back into the part of the billet that has not been extruded yet. There is no closed-form solution to the combined conduction problem; the published treatments solve it numerically, with finite differences on a gridded meridian plane of the billet and boundary conditions at the container wall, the dead-metal cone, the dummy interface and the die exit.
What matters on the shop floor is the direction of the imbalance. Exit temperature rises when heat production from deformation and friction exceeds the losses, and falls when it does not. Heat conduction takes time, which is why heat production wins above a certain ram speed, and why the exit temperature profile along a single extrusion changes as the stroke proceeds.
The five variables that move the exit temperature
| Variable | Effect on exit temperature | Why |
|---|---|---|
| Material flow stress | Higher flow stress, more heat | Dissipated deformation heat is proportional to flow stress at the given strain and strain rate |
| Friction | More friction, more heat at the wall and the dead-metal zone | Temperature rise is proportional to the friction shear stress |
| Ram speed | Rises with speed, apparently linearly | Strain rate is proportional to ram speed, and generated heat to strain rate |
| Extrusion ratio | Higher ratio, higher exit temperature | More severe plastic deformation at higher strain |
| Outside perimeter | Larger perimeter, higher exit temperature | The bearing friction area is perimeter times bearing length |
The published variables and their direction of effect. The perimeter entry is the one most often left out of a press setting sheet, because it belongs to the die rather than to the press.
Two counters that surprise people
In a controlled series on thin-gage 6063 square tube — 152 mm billet, 162 mm container bore, extrusion ratio 90, die starting at 440 °C, blended bearing 2.0 to 3.5 mm — the measured exit temperature rose with ram speed in every case, apparently linearly. The two variables that were not ram speed behaved in ways worth remembering.
Billet length. A longer billet raised the exit temperature more than a change in ram speed did, because a longer billet means a longer cycle, and a longer cycle means more container friction to overcome. The press has been pushing the same billet past the same liner for longer, and the metal pays for it in temperature.
Bearing surface condition. A new nitrided bearing ran cooler than an old one. The mechanism is friction type, not finish: a new, hard nitrided bearing sticks less to the aluminum and slides more, so the friction stress — and the heat it produces — is lower. An old bearing with aluminum buildup is closer to sticking friction, and the exit temperature rises accordingly. That is the same adhesion that produces pick-up on a 6xxx profile, seen from the thermal side, and it is described on the pick-up and die lines page.
The measured exit temperatures also matched a finite-difference model of the same runs to within 2 to 4%. For a shop, that is the useful part of the result: the model is good enough to plan a speed with, and a single contact reading at the end of the stroke is good enough to confirm it.
Where to measure it, and what each method can see
| Method | What it gives | What limits it |
|---|---|---|
| Thermocouple buried in the die | Die body temperature, well below the bearing | Response too slow to catch a rapid change; reads the die, not the metal |
| Thermocouple in the bearing itself | The true surface temperature of the profile | Scraps the profile; a laboratory method, not production practice |
| Contact probe on the runout table | A spot reading, accurate if the probe is perpendicular and the metal is stopped or very slow | Needs 3 to 4 s of holding time; probe oxidation and wear; discontinuous, so it cannot profile a stroke |
| Noncontact infrared pyrometer | Continuous reading from start to end of the stroke | Emissivity of aluminum changes with surface condition; multiwavelength compensation keeps the error under 1% |
| Eddy-current sensor | Average temperature through the penetration depth, and area | Gives a bulk average, not the surface peak; ±5 °C at 538 °C in the published trial |
Measurement methods compared. The two that can drive a control loop are the noncontact ones, because the loop needs a continuous signal, not a spot reading.
One finding from the same work is worth carrying into the plant: thermocouples in the die and readings taken on the runout table differ greatly. The die temperature is not the extrusion temperature, and readings taken at the centre of a profile are consistently higher than those at the edges or in the corners. A shop that holds one probe against one face and calls it the exit temperature is measuring the coolest part of the section.
Isothermal extrusion: hold the exit, not the ram
Run a constant ram speed and the exit temperature still moves: it rises toward the start and the end of the stroke for a given billet, container and die. Isothermal extrusion is the practice of varying the ram speed to hold the exit temperature constant instead. Its value is economic before it is metallurgical — if the exit temperature varies by an unknown amount, the press speed has to be set for the hottest point of the cycle, and there is wasted speed capacity everywhere the exit is cooler.
Three ways to do it appear in the published literature, and they can be combined:
- Reduce the exit speed as the measured exit temperature rises — needs a continuous temperature signal.
- Reduce the speed on a pre-set program, dividing the ram displacement into steps of varying length, each with its own speed.
- Taper heat the billet so the back end starts cooler: induction coils connected to heat the front harder, extra burners in a gas furnace, or uniform heating followed by a water spray on the back end as the billet travels to the container.
The two methods that survive in industry are taper heating or taper quenching before the container, and direct measurement of the extrusion temperature with feedback to the ram speed. Both are older than the control hardware now used to run them: a taper quench unit for production was built for billet diameters from 178 to 381 mm, and a press set up with a zoned working stroke — each zone with a preset speed — claimed a 60% time saving on high-strength alloys, with less to gain on easy alloys. A later industrial installation reported productivity up to 23% higher with constant exit temperature.
The practical caution attached to all of it is that these systems only pay if the plant runs efficiently and the operating team is watching the result. A closed-loop speed control on a press that is late, cold or badly tooled moves the problem rather than solving it.
What the exit temperature does to the die
Exit temperature has two distinct effects in the published treatment, and only one of them is about the product. On the product side it sets the quench and ageing result, the dimensional stability and the defect population. On the die side it sets wear, and it does so through the bearing: the local temperature rise at the bearing is what changes the adhesive layer on it, and a changing adhesive layer changes both the friction and the metal flow through the land.
That is why the bearing temperature drifts upward as a run proceeds even when the press settings do not change, and why the die’s condition at the end of a shift is not the condition it started with. Nitrogen or water cooling on the die, and nitrogen on the bearing, are the direct countermeasures; a harder bearing surface is the indirect one, because it lowers the friction stress in the first place.
Where this leaves a die steel order
Two of the findings on this page land on the die material rather than on the press. The first is that bearing temperature and bearing hardness are the same question: the die has to hold its hardness at the temperature the land actually reaches, which is what the working hardness and tempering on the H13 tool steel page are for. The second is that a hard, nitrided bearing runs cooler than a soft one, which is the case for the case on the tool steel nitriding page.
The rest of the cluster: the extrusion die grade and its ESR supply on the 1.2344 ESR H13 page, the bearing length that sets the friction area on the die bearing length page, the wear that follows a long run on the die wear page, the grade comparison on the best tool steels for extrusion dies page, and the effect of a hotter or cooler die face on the section in die correction.
Before you set a speed from this page
These are the published mechanisms and the published measurements on one alloy in one plant, not a speed table. The exit temperature a given die will produce depends on the alloy, the section, the container, the billet length and the condition of the bearing, and it changes as the bearing wears. Establish the profile at constant speed first, then decide whether a taper or a feedback loop is worth installing.
Source, Aluminum Extrusion Technology, P. K. Saha, ASM International, 2000, chapter 2, thermodynamics in extrusion and isothermal extrusion, pages 30 to 46.