Press Quench and Aging: Why the Same 6061 Shape Tests Different Along Its Length
Between the die and the age oven there is a cooling step that decides whether the section can reach its temper at all. For 6xxx it usually happens on the runout: fans, sometimes water, pulling the metal down from the exit temperature fast enough to hold the hardening elements in solid solution. Do it unevenly and the same profile passes its tensile test at the front and fails it at the back, because the strip at the far end of the table cooled at a different rate from the strip under the first fan. This page covers what the quench has to achieve, when a fan is not enough, what the aging oven does afterwards, and how the test results are read back into the process.
What the quench is for
The hardening phase of a 6xxx alloy is Mg2Si. For the alloy to respond to aging, that phase has to be taken into solution at the exit temperature and then kept there by cooling fast enough that it does not precipitate as coarse particles on the way down. The quench at the press is therefore a solid-solution treatment followed immediately by a cooling rate, and if either half is missing the aging oven cannot recover it.
| Alloy group | Principal hardening phase |
|---|---|
| 1xxx | FeAl3, Fe2SiAl5 |
| 3xxx | MnAl6, (FeMn)Al6 |
| 5xxx | Mg2Al3 |
| 6xxx | Mg2Si |
Principal hardening phases of the soft and medium-grade alloy groups. The 5xxx phases harden by work and the 6xxx phase by precipitation, which is why only one of them needs a quench.
Air first: what a fan bank has to do
For 6xxx the extrusion may be cooled directly from the extrusion temperature, and a forced-fan system is normally sufficient. Water is the exception rather than the rule. The heat transfer depends on two things only: the air velocity and the air temperature at the surface of the extrusion.
That sounds trivial until the uniformity requirement is applied. The published condition for uniform mechanical properties over the full length of the product is that the air velocity along the axis of the press equals the air velocity at the first section of the cross-transfer conveyor. In other words the section must not leave the high-velocity zone and coast through still air at the transfer point — because the metal that cooled slower there is the metal that will fail the test. Enough fans, at enough velocity, to reach the cooling intensity the thickest wall of the order needs.
Whether air is enough depends on two variables, and only two: the thickness of the section and the alloy with its chemistry. A thin, light section can be air quenched at the press provided it leaves the die above the solid-solution temperature. A heavy one has to be checked rather than assumed.
When the press cannot do it at all
The case that catches 6061 structural work is thermal, not metallurgical. A heavy section with a low extrusion ratio may never reach the solid-solution temperature on its way through the die, so no quench at the press — air or water — can complete the solution treatment, because there was nothing to retain. The answer is a separate solution heat treatment in a furnace, followed by a controlled quench.
- Horizontal furnace with a water-jet quench
- Vertical furnace with a water-tank quench
- Controlled-volume, full-immersion water or glycol solution quench in either type
- Polymer glycol as an alternating medium to water, to reduce distortion
After a furnace solution treatment the extrusions are stretched to straighten them and to release the internal stresses the quench put in — 1.5 to 3% is the published figure for that duty, which is slightly more than the 1 to 3% used for ordinary straightening and is chosen for stress relief rather than shape alone.
Aging, and the oven survey
Aging is the final stage, and it is where the temper is actually made: hardness, strength and ductility are set by the temperature, the time, and the uniformity of the load. The published practice numbers are below. They move with the specification and the supplier, and the shape of the table is more useful than the individual cells — solution temperature around 520 to 545 °C, aging between 160 and 180 °C, between 6 and 18 hours depending on the alloy and the temper.
| Alloy | Solution, °C | After quench | Aging, °C | Aging time, h | Final temper |
|---|---|---|---|---|---|
| 6005 | 530 | T1 | 175 | 8 | T5 |
| 6061 | 530 | T4 | 175 | 8 | T6 |
| 6063 | 520 | T4 | 175 | 8 | T6 |
| 6063 | 520 | T4 | 182 | 6 | T6 |
| 6066 | 530 | T4 | 180 | 8 | T6 |
| 6070 | 545 | T4 | 160 | 18 | T6 |
| 6262 | 540 | T4 | 175 | 12 | T6 |
Typical heat treatment practices for 6xxx alloys. The 6063 alloy appears twice because two aging combinations reach T6, which is the point: the specification sets the practice, not the alloy name.
The one maintenance instruction that comes with the table is about the oven itself. A published survey of aging oven performance used up to 32 thermocouples in a single typical load to map the temperature profile, and the recommendation that follows from it is to survey each aging oven at least once a year. An oven that is 5 °C out at one corner does not fail anything on the day it drifts; it produces a section that passes, then a section that is marginal, then a customer complaint with no obvious cause.
How the result is tested, and what the test tells the press
For 6063 architectural and decorative shapes, hardness is the only qualifying test most extruders run. For industrial and structural work, tensile testing is required, and for structural shapes the set is tension, compression and shear. Samples are normally taken from the back end of an extrusion — sometimes from the front, middle and back, precisely to establish how much the properties vary along the length.
The macro-etch is the test that feeds back into the process rather than into the certificate. Etching the back end, and the same three positions, shows the grain structure in the recrystallized regions — usually around the periphery of the profile or at the tips of thin legs — and it shows entrapped inclusions at the back end. If the etch finds them, the fix is not in the aging oven: it is a thicker butt, or a correct temperature differential between billet and container so that the oxide skin stays in the container instead of being drawn into the section. Both are set out on the butt thickness and yield page.
Hardness is also the cheapest process control the line has. A hardness reading that drops at the back end of a run is telling you that either the quench at that point is weaker than at the front — the fan uniformity problem — or the butt is thin enough that back-end metal is in the section.
Where this leaves a die steel order
The quench and the aging oven belong to the extruder, but the section that arrives there was cut by a die, and two die-side decisions show up in the test results. The first is exit temperature: if the metal leaves the die below the solid-solution range, no press quench can put the alloy into condition, and the answer is a lower extrusion ratio, a hotter billet or a furnace route. The second is the condition of the bearing: a worn or built-up land raises the exit temperature locally and changes the surface the quench sees first.
For the die stack itself, the grade and its heat treatment are on the H13 tool steel page and the extrusion programme on the 1.2344 ESR H13 page; the land on the die bearing length page; the surface treatment that follows a correction on the tool steel nitriding page; and the window the exit temperature has to stay inside on the die temperature and isothermal extrusion page.
Before you set a quench from this page
Cooling rate is set by the section, the alloy and the equipment on the line, and the published temperatures in the table above are starting points, not a schedule. What transfers between plants is the logic: air velocity and its uniformity, thickness against the quench medium, the solid-solution temperature before the quench, and an oven survey once a year. Test the back end, and read the variation along the length before adjusting anything.
Source, Aluminum Extrusion Technology, P. K. Saha, ASM International, 2000, chapter 6, heat treatment, mechanical and physical tests, pages 175 to 179.