Bulk tool steel bar stock in the Aobo Steel warehouse

5CrNiMo Tool Steel

AOBO STEEL – Trusted Global Tool Steel Supplier

5CrNiMo steel is a traditional low-alloy hot-work tool steel that has been widely used in various applications, particularly for forging dies. It has excellent hardenability, good toughness, and moderate strength at elevated temperatures, though it has some limitations in very high-temperature or high-wear applications. 5CrNiMo is a grade under China’s GB/T standard, with equivalent grades including American AISI L6, Japanese JIS SKT4, and German DIN W-Nr. 1.2713 and 1.2714.

1. Chemical Composition of 5CrNiMo Steel(GB / T 1299—2000)

CSiMnCrNiMoPS
0.50-0.60≤0.400.50-0.800.50-0.801.40-1.800.15-0.30≤0.030≤0.030

2. Physical Properties of 5CrNiMo

2.1 Critical Temperature of 5CrNiMo

Critical PointAc1Ac3Ar1Ar3Ms
Temperature/ °C730780610640230

2.2 Linear Expansion Coefficient of 5CrNiMo

Temperature / °C100 ~ 250250 ~ 300350 ~ 600600 ~ 700
Linear Expansion Coefficient α / x10⁻⁶ °C⁻¹12.5514.114.215.0

2.3 Elastic Modulus of 5CrNiMo

Temperature / °CRoom Temp100200300400500
E / MPa209 720206 780203 840198 940193 060186 200

2.4 Shear Modulus of 5CrNiMo

Temperature / °CRoom Temp100200300400500
G / MPa83 30082 32080 36078 40075 46073 500

2.5 Thermal Conductivity

Temperature / °CRoom Temp100200300400500
λ / [W / (m · K)]0.440.440.430.430.390.35

2.6 Specific Heat Capacity

Temperature / °CRoom Temp ~ 100Room Temp ~ 200Room Temp ~ 300Room Temp ~ 400Room Temp ~ 500
cₚ (20°C) / [J / (kg · K)]0.4840.4970.5090.5310.552

2.7 Density is 7.804 g/cm³.

3. Hot Forging Process Specification of 5CrNiMo

ItemHeating Temperature / °CInitial Forging Temp. / °CFinal Forging Temp. / °CCooling Method
Steel Ingot1140 ~ 11801100 ~ 1150800 ~ 880Slow cooling (pit or sand cooling)
Steel Billet1100 ~ 11501050 ~ 1100800 ~ 850Slow cooling (pit or sand cooling)

Note: 5CrNiMo steel can be hardened by cooling in air, but it is prone to forming white spots, so it should be cooled slowly after forging. For large forgings, they must be held in a furnace at 600°C until the temperature is uniform, then slowly cooled to 150-200°C, and finally cooled in air. For larger forgings, tempering should be carried out immediately after cooling to 150-200°C.

5CrNiMo
5CrNiMo steel

Please complete the following contact form to receive the most accurate quotation for 5CrNiMo steel.

    4. Heat Treatment of 5CrNiMo

    4.1 Preheating

    ① Post-Forging Annealing Options

    Preliminary Heat Treatment OptionProcess Parameters
    Post-Forging AnnealingHeat to 760–780°C, hold for 4–6 hours, then cool the furnace to below 500°C before unloading for air cooling. After annealing, the hardness ranges from 197 to 241 HBW, with a microstructure of pearlite + ferrite.
    Post-Forging Isothermal AnnealingHeating temperature: 850–870°C, held for 4–6 hours; Isothermal temperature: 680°C, held for 4–6 hours; Cooled in the furnace to below 500°C, then removed for air cooling; Post-annealing hardness: 197–241 HBW; Microstructure: pearlite + ferrite.
    Forging Die Renewal AnnealingHeat to 710–730°C, hold for 4–6 hours, then cool in the furnace to below 500°C before removing for air cooling. Post-annealing hardness: 197–241 HBW.

    ② Microstructure and Hardness Before and After Annealing

    Indentation Diameter / mmHBWMicrostructure (Before Annealing)Microstructure (After Annealing)
    3.9 ~ 4.3241 ~ 197Troostite + MartensitePearlite + Ferrite

    4.2 Quenching

    ① Recommended Quenching Process Specification

    Quenching Temperature/°CQuenching Cooling MediumQuenching Cooling Medium Temperature/°CContinuedHardness HRC
    830 ~ 860Oil20 ~ 60Temper immediately after cooling to 150 ~ 180°C53 ~ 58

    Note:

    • For large molds, use the upper limit for quenching heating temperature; for small molds (side length below 200–300 mm), use the lower limit.
    • To minimize stress and deformation during quenching, after heating to 830–860°C, first pre-cool in air to 750–780°C, then oil-quench to 150–180°C. Remove and immediately temper.
    • For large molds, slowly heat to 600–650°C and hold for 1–1.5 hours. Only increase furnace temperature after thorough heating. To improve heating quality, place workpieces on 60–100mm thick backing plates during heating.
    • Module quenching at low oil immersion temperatures increases cracking risk. To prevent cracking, actual practice often involves oil immersion around 200°C. While this produces a martensitic surface layer, the core remains in the austenitic state. To extend service life, isothermal quenching can be employed.

    ② Isothermal Quenching Process

    Process TypeQuenching Temp. (°C)Cooling MediumMedium Temp. (°C)Isothermal Temp. & TimeQuenching Hardness (HRC)Microstructure after Quenching
    Isothermal Quenching830 – 860Oil20 – 60Cool mold surface to 150-200°C, then hold in a 280-300°C bath for 2-3h–Small amount of bainite + lower bainite + retained austenite. After tempering, bainite transforms to lower bainite.
    High-Temp Quenching890 – 910Oil––61.5Lath martensite + retained austenite (approx. 9.2% by volume), grain size 7-8.

    Notes:

    • Isothermal Quenching: This process reduces the tendency for the mold to crack and improves its service life.
    • High-Temperature Quenching: Tempering temperature is 420-550°C, tempered twice, resulting in a hardness of 38-47 HRC.

    4.3 Tempering

    ① Recommended Tempering Process Specifications

    PlanTempering PurposeForging Die SpecificationTempering Temperature (°C)Heating EquipmentHardness (HRC)
    IEliminate stress, stabilize structure and sizeSmall490 ~ 510Gas furnace or Electric furnace44 ~ 47
    Medium520 ~ 54038 ~ 42
    Large560 ~ 58034 ~ 37
    IIDovetail (Medium)620 ~ 64034 ~ 37
    Dovetail (Small)640 ~ 66030 ~ 35

    Note: After tempering, oil quenching should be performed to prevent the development of temper brittleness. To relieve stresses generated during oil quenching, a second tempering at 160–180°C may be conducted. Large forging dies must not be cooled to room temperature in oil during either quenching or tempering, as this may cause cracking.

    ② Effect of Quenching and Tempering Temperatures on Impact Toughness

    Tempering Temp. (°C)300350400450500
    Quenching Temp. (°C)840The values in the table represent impact toughness, a_k / (J/cm²).2125293545
    Quenching Temp. (°C)9501920232535
    Quenching Temp. (°C)10001316202330

    Note: When the 5CrNiMo steel module is tempered at 380-450°C, the supercooled austenite in the core transforms into an upper bainite structure, resulting in extremely poor impact toughness.

    ③ Effect of Quenching and Tempering Temperatures on Hardness of 5CrNiMo

    Tempering Temp. (°C)300350400450500550600
    Quenching Temp. (°C)850Hardness HRC52504845413832
    Quenching Temp. (°C)90052504845413832
    Quenching Temp. (°C)95053514946423933
    Quenching Temp. (°C)100054525047434034

    5. Mechanical Properties

    5CrNiMo steel is a traditional hot-forging die steel, exhibiting good plasticity and toughness alongside adequate strength and wear resistance. It is insensitive to size effects, with room-temperature mechanical properties nearly identical to those at temperatures ranging from 500 to 600°C. When heated to 500°C, it still maintains a hardness of approximately 300 HBW. Due to its low content of carbide-forming elements, the secondary hardening effect is weak, resulting in poor thermal stability and low high-temperature strength.

    5.1 High-Temperature Hardness of 5CrNiMo

    Temperature (°C)300450600650710750
    Hardness (HV)383351 ~ 354254 ~ 274201 ~ 203147 ~ 15471.3 ~ 72.7

    5.2 High-Temperature Impact Toughness of 5CrNiMo

    Temperature (°C)300600650700
    Impact Absorption Energy (KU/J)48.436.436.370.3

    5.3 Thermal Fatigue Performance

    Test Method & State20°C ←→ 650°C (1000 cycles)20°C ←→ 750°C (1000 cycles)
    Level¹13.420.0

    ¹The higher the level, the worse the thermal fatigue performance.

    5.4 Thermal Wear Performance

    Number of Revolutions300600900120015002500
    Weight Loss / mg1.002.433.274.24.975.97

    Note: Using the S. R. Tittagala method, at a temperature of 800 ~ 850°C and a pressure of 784~850N.

    5.5 Surface mechanical properties and core mechanical properties

    PartLocationRm/ MPa(Tensile Strength)Rel/ MPa(Yield Strength)A (%)(Elongation)Z (%)(Reduction of Area)KU/J(Impact Energy)
    Room TempSurface1310––4131.3
    Room TempCore1020761164214.1
    300°CSurface1214––5848.4
    300°CCore1011833266259.2

    Note: During quenching of large-section workpieces, differing cooling rates between the surface layer and the core result in distinct mechanical properties. This phenomenon in steel is termed the mass effect, also known as the size effect.

    6. Applications

    5CrNiMo steel, due to its excellent hardenability, exhibits nearly uniform hardness across its cross-section when large blocks (300mm × 400mm × 300mm) undergo quenching in oil at 820°C followed by tempering at 560°C. Primarily used for manufacturing various small and medium-sized forging dies with side lengths ≤300mm and operating temperatures below 500°C. It is more suitable for producing large and medium-sized modules in mass production, and can also be used to fabricate complex-shaped casting mold components.

    1.2714
    1.2714
    5CrNiMo
    5CrNiMo