Aobo Steel | Global Tool Steel Supplier in China
AISI D6 Tool Steel | 1.2436 | SKD2 Tungsten-Alloyed Cold Work Steel
- 100% UT Tested Quality Assurance
- SEP 1921-82 Class D/d Guaranteed
- Annealed State Delivery
- Surface: Black Scale, Turned, Mill Finish, or Polished
D6 Tool Steel is classified under the AISI system as a high-carbon, high-chromium cold-work tool steel. Steels in this category typically have a nominal chromium content of around 12%, which is fundamental to their performance. The specific properties are fine-tuned by varying alloying elements, such as carbon, molybdenum, vanadium, and manganese.
1. Applications
- Long production run blanking dies
- Cold-forming punches and dies
- Tooling components subjected to severe abrasion
- Applications where maintaining a sharp edge over extended use is critical
2. D6 Steel Composition
| Carbon (C) | Chromium (Cr) | Tungsten (W) | Manganese (Mn) | Silicon (Si) |
| 2.00 – 2.20% | 11.50 – 12.50% | 0.60 – 0.90% | 0.20 – 0.40% | 0.10 – 0.40% |
The D6 tool steel equivalent grades’ composition
| Carbon (C) | Silicon (Si) | Manganese (Mn) | Chromium (Cr) | Tungsten (W) | Phosphorus (P) | Sulfur (S) | |
| Germany/W-Nr. 1.2436 (X210CrW12) | 2.00 – 2.30% | 0.10 – 0.40% | 0.30 – 0.60% | 11.0 – 13.0% | 0.60 – 0.80% | ≤ 0.030% | ≤ 0.030% |
| Japan/JIS SKD2 | 2.00 – 2.30% | 0.10 – 0.60% | 0.30 – 0.60% | 11.0 – 13.0% | 0.60 – 0.80% | ≤ 0.030% | ≤ 0.030% |
| China/GB Cr12W | 2.00 – 2.30% | ≤ 0.40% | ≤ 0.40% | 11.0 – 13.0% | 0.60 – 0.90% | ≤ 0.030% | ≤ 0.030% |
3. Properties of D6 Steel
3.1 Physical properties
| Density | Thermal Expansion Coefficient | Thermal Conductivity | Specific Heat Capacity |
| 7.67 g/cm³ | 10.8 µm/m°C (21-400°C) | 20.5 W/mK (20°C) | 0.460 J/g-°C (20°C) |
3.2 Hardness and Wear Resistance
A primary advantage of D6 Tool Steel is its very high wear resistance. This stems directly from its high carbon and chromium content, which promotes the formation of hard chromium-rich carbides in the steel’s microstructure after heat treatment. Properly hardened and tempered, D6 typically achieves a hardness of 54-61 HRC. Its wear resistance generally exceeds that of the more common D2 tool steel, making it suitable for applications that demand a long service life under abrasive conditions.
3.3 Toughness
D6 has high wear resistance, but lower toughness. Compared with shock-resistant steels (such as S-series) or other cold-work steels with lower carbon content (such as A-series or D2), D6 Tool Steel is more brittle. The same hard carbides that resist wear can make the steel more prone to chipping or cracking under impact. Therefore, D6 Tool Steel is not recommended for applications involving significant shock or impact loading.
3.4 Hardenability and Heat Treatment
D6 is a deep-hardening steel; it can achieve relatively uniform hardness through its cross-section, even in larger sizes. It is typically an oil-hardening grade, though it can be air-hardened at the expense of achievable hardness. Tempering after hardening is essential to relieve stresses and achieve the desired balance of hardness and toughness.
3.5 Dimensional Stability
As an oil-hardening steel, D6 may exhibit greater dimensional changes during heat treatment compared to air-hardening grades like D2 Tool Steel. Careful control of the heat treatment process is necessary if tight dimensional tolerances are critical.
3.6 Machinability and Grindability
Due to its high hardness and significant carbide content, D6 steel is considered more difficult to machine and grind compared to lower-alloy steels or even D2. This should be factored into manufacturing processes and costs.
4. D6 tool steel heat treatment
4.1 Preheating
Preheating reduces thermal shock, thereby lowering the risk of subsequent cracking or deformation. Preheating is typically performed at temperatures between 650°C and 760°C (1200°F and 1400°F). Ensure that the entire tool has reached the preheating temperature uniformly before calculating the soaking time. Based on our experience, the soaking time is 10–15 minutes.
4.2 Austenitizing (Hardening)
The purpose of this step is to transform the steel’s microstructure into austenite, preparing it for subsequent quenching. The temperature range is 950°C to 1050°C (1740°F to 1920°F). The holding time is 1 hour per 25 mm (1 inch) of thickness. It is important to note that insufficient holding time may result in incomplete quenching, while excessive holding time may lead to grain growth and reduced toughness.
4.3 Quenching
This step involves transforming the austenite into hard martensite. D6 Tool Steel is an oil-hardening steel. Oil quenching provides a sufficiently fast cooling rate for hardening while being less harsh than water, which significantly reduces the risk of cracking and distortion.
The specific process involves quenching the workpiece in oil until it cools to room temperature or to 65 °C (150 °F).
Sometimes, air-quenching is also chosen, but the hardness after air quenching is relatively lower. If higher deformation requirements are specified, air quenching of D6 steel can be considered.
4.4 Tempering
The purpose of tempering is to reduce brittleness and increase toughness. A two-step tempering process is recommended to ensure maximum stress relief and dimensional stability.
The tempering temperature ranges from 150°C to 550°C (300°F to 1020°F). The soaking time is 2 hours per 25mm (1 inch) of thickness for each tempering cycle.
The tempering temperature determines the material’s final hardness. Higher tempering temperatures reduce the hardness of D6 steel but increase its toughness. The specific temperature should be determined based on actual application requirements.
Table of Hardness and Tempering Temperature for D6 Steel
| TEMPERING TEMPERATURE | Rockwell C |
| As quenched | 67 |
| 300°F / 150°C | 65 |
| 400°F / 205°C | 64 |
| 500°F / 260°C | 63 |
| 600°F / 315°C | 62 |
| 700°F / 370°C | 61 |
| 800°F / 425°C | 61 |
| 900°F / 480°C | 58 |
| 1000°F / 540°C | 55 |
4.5 Achieving Better Results and Avoiding Problems
Proper process control is crucial to achieving a successful heat treatment.
4.5.1 Dimensional Stability
To reduce the risk of D6 steel deformation during quenching, the following precautions should be taken.
- Two preheating cycles can be performed.
- Ensure uniform heating during the austenitization process.
- Stir during oil quenching.
- Perform stress-relief treatment after rough machining and before the final heat treatment.
4.5.2 Stress Relief (Post-Hardening)
Stress relief treatment should be performed after heavy grinding, welding, or electrical discharge machining. The stress relief temperature should be 15°C to 30°C (25°F to 50°F) lower than the final tempering temperature. The holding time should be 1-2 hours per 25mm (1 inch) of thickness.
4.5.3 Common Heat Treatment Issues
- Cracking: Often caused by thermal shock (insufficient preheat or excessively harsh quench).
- Distortion: Caused by non-uniform heating/cooling or internal stresses.
- Inadequate Hardness: Results from incorrect austenitizing temperature/time or insufficient quenching.
4.6 Forging D6 tool steel
Slowly preheat to 900 °C (1650 °F). Forging should begin within the temperature range of 980 °C (1800 °F) to 1095 °C (2000 °F). Do NOT forge below 900 °C (1650 °F). For larger cross-sections, heavier pieces, or rapid thinning, use the higher end of the temperature range; for smaller cross-sections or lighter thinning, use the lower end.
5. Comparison with Other Tool Steels
5.1 D6 vs. D2
D2 and D6 tool steels are high-carbon, high-chromium cold-work tool steels known for their wear resistance. D6 has slightly higher wear resistance at the cost of lower toughness and more complex/difficult heat treatment (oil quenching, higher distortion risk). D2 is more widely used due to its better balance of properties, especially its air-hardening capability and minimal distortion.
5.2 D6 vs. D3
- Both are high-carbon, high-chromium, oil-hardening steels renowned for their exceptionally high wear resistance.
- Minor compositional differences may exist (sometimes W or V in D6 Tool Steel).
- D3 heat treatment is more complex than D6.
5.3 D6 vs. D7
- D7 contains added vanadium, potentially offering even higher abrasion resistance than D6 Tool Steel.
- D7 typically has lower toughness than D6 and requires higher hardening temperatures.
6. Considerations When Choosing D6 Tool Steel
D6 steel is an excellent choice for applications that demand maximum wear resistance in cold-work tooling. However, carefully consider:
- Lower Toughness: Not suitable for high-impact applications.
- Processing: More challenging to machine and grind.
- Heat Treatment: Oil quenching requires careful process control for dimensional stability.
- Availability: May be less readily available than D2 Tool Steel.
7. Equivalent Grades
- DIN EN (Europe): 1.2436 (X210CrW12)
- JIS (Japan): SKD2
- BS (UK): BD6
- ISO: X210CrW12
- GB(China): Cr12W
8. Supply forms and dimensions
The D6 tool steel that we supplied is in various forms, including round bars, sheet plates, slabs, flat bars, square bars, and blocks. The dimensions of the flat bar range from: width 20–600 mm × thickness 20–400 mm × length 1,000–5,500 mm. The dimensions of the round bar range from a diameter of 20–400 mm × a length of 1,000–5,500 mm. The block dimensions are obtained by cutting the flat bar.
For smaller sizes, such as round bars with a diameter less than 70 mm, we use the hot-rolled process. For sizes greater than 70 mm, we offer forged products.
UT testing: Sep 1921-84 D/d, E/e.
Surface Treatment: original black, peeled, machined/turned, polished, grounded, or milled surface finishes.
Inventory Status: We do not maintain a stock of D6 steel. We arrange production based on customer orders.
Delivery time: Electric Arc Furnace (EAF) materials are 30-45 days. ESR materials are approximately 60 days.