Butt Thickness, Runout and Recovery: Where the Yield of an Aluminum Extrusion Is Decided
Two numbers decide what a press earns on a billet: how many metres come out of it, and how much metal is left in the container when the ram stops. They are the same decision seen from two sides. Leave a thin butt and the runout looks good per billet, but the back end carries the oxide, the radial flow and sometimes a flare. Leave a thick butt and the yield falls on every billet of every order, all year. This page covers the arithmetic of runout, the published butt practice for critical sections, and the two failure modes — back-end defects and flare — that punish a butt set too thin for the shape.
The wall thickness and press-size limits for a given circumscribing circle are on the circumscribing circle diameter page; that page notes that a larger CCD needs a thicker butt, and this page is the rest of that argument.
Runout: volume constancy, and the estimate that pays for itself
The metal that leaves the container has to equal the metal that arrives at the die, less what stays behind as the butt. Written as volume constancy:
AC × LB = AE × LR, where AC is the container bore area, LB the effective billet length, AE the cross-sectional area of the extrusion and LR the runout length. The effective billet length is the billet length minus the butt, and the ratio AC/AE is the extrusion ratio, so the runout is simply the extrusion ratio multiplied by the usable billet length.
That identity is enough to quote a run before the die is on the press. On a 178 mm container bore at an extrusion ratio of 20, a usable billet length of 450 mm gives 9.0 m of runout. Raise the ratio to 30 on the same billet and the estimate is 15.0 m — with a section one third the area. Both numbers come from the die print, which is why the die print is the document the production planner needs first.
In the shop the same figure is measured by weight, because the real section area drifts from the drawing. Runout is the billet weight minus the butt weight, divided by the actual weight per unit length of the extrusion. The two methods answer different questions: the die-print estimate tells you whether the order fits the runout table, the weight measurement tells you what the die actually produced.
The calculated and the measured figure differ for reasons worth listing, because each one is a knob someone owns: contraction of the metal as it leaves the bearing, which depends on billet temperature and speed; the die design and its support tooling; puller tension; thermal contraction on the cooling table; and the alloy. With a puller in the line the extrusion is being stretched while it is still hot, so the exit speed without puller tension, ram speed times extrusion ratio, is not the speed the runout table sees.
The same die, the same billet, a different runout
Run thin-gage 6063 through one die at a fixed billet length, billet temperature and butt thickness, and the runout still moves. Four published causes account for it:
- Die deflection
- Extrusion ratio
- Extrusion speed
- Number of billets run
The fourth one is the one that catches quality people out, and the reason is thermal. The billet is at its hottest at the die exit, close to the die corner. Heat passes from the billet into the die and the tooling and from there to the air, so the die takes time to reach steady state for a given billet temperature, billet length and extrusion ratio. Until it does, its temperature — and therefore its hardness — is still changing.
The deflection follows. At extrusion pressure and temperature the die face bows, the opening closes, and the profile comes out undersized; the bowing is greatest at the centre of the die and falls off toward the periphery, which is exactly the thickness variation seen across a profile. Hotter die, lower hardness in the H13 die steel, more deflection — which is why the same die produces a slightly different section on the first billet of a run and on the tenth, and why the runout length moves with the billet count.
The sensitivity is larger than most people assume. A 4.0% reduction in wall thickness at the centre of the profile increases runout by about 2.5% through volume constancy alone. On a 2.0 mm wall that is 0.08 mm of section, and it is the difference between a die that is running correctly and a die that is being blamed for a press problem.
Setting the butt: what the book actually says
The butt is set per die and per order, and the published guidance is narrower than the range of practice. For critical sections — structural work, where a back-end defect can start a longitudinal crack at a load far below the design load — butt thickness of 10 to 20% of the billet is typical, and an etch test on the back end is recommended to confirm that no inclusion or defect has been drawn into the section. On a 500 mm billet that is a 50 to 100 mm butt, and it is metal the customer does not buy.
| What the butt setting controls | If the butt is too thin | If the butt is too thick |
|---|---|---|
| Back-end quality | Oxide from the billet skin is drawn into the section as an annular ring or internal pipe; piping and funnels open at the back face | Sound, but at the cost of metal |
| Shape at the end of the run | Wide sections go wavy toward the end | Waviness controlled — this is the published fix |
| Container sealing | Sealing pressure alone holds the liner to the die face; flare risk rises | Friction drag maintained to the end of the stroke |
| Yield | Higher recovery per billet | 10 to 20% of the billet lost on critical sections |
The butt is a quality variable and a yield variable at the same time; it cannot be optimized on one axis alone. Butt percentages follow the published practice for critical sections.
Flare: the failure that arrives when the butt gets thin
Flare is a soft-alloy problem and it is a butt problem. At the start of the stroke the container liner is held against the die face by two things: the sealing pressure of the press, and the friction drag of the billet sliding in the liner. As the billet shortens, the friction drag falls to a minimum, and by the time the ram approaches the set butt thickness the seal is being held by sealing pressure alone. At the same time the remaining metal is more plastic, because its temperature has risen during the stroke. If there is a gap between the die face and the liner, that plastic metal back-extrudes through it.
Three conditions open the gap, and all three are inspectable before the run: aluminum buildup on the liner face or a worn liner face; a die diameter smaller than the outside diameter of the liner, which indents the liner face over time; and sealing pressure that is not what the press thinks it is. The published fix in the short term is to keep a thicker butt until the container is replaced; the durable fixes are the correct die diameter, a clean liner face, and a periodic check of sealing pressure. The liner, the dummy pad and the clean-out block that sit in this joint are described on the container liner and dummy block page.
Flare is also the reason a butt cannot be judged in isolation from the container. A shop that has just replaced a liner, or is running a die whose outside diameter is a little under the liner OD, will flare at a butt thickness that was safe last month.
Feeder plate and recessed dies: the first two billets are different
On a feeder plate or a recessed die, the pocket has to keep aluminum from the previous billet so that the next billet welds to it and the extrusion stays continuous. A thick butt pulls aluminum out of that pocket, and on the first one or two billets — before the die reaches thermal steady state — that is exactly when the pocket is easiest to empty. The result is preferred adhesion of aluminum into the pocket and a die that runs differently from the third billet onward. It is the same thermal story as the deflection, seen from the die’s point of view.
Recovery is a control chart, not an annual report
Productivity is good extrusion per unit time, and the published levers are three: minimize avoidable scrap per billet run at the same press speed, billet size and runout length; maximize billet length to use the press capacity and the runout table; and optimize speed while compensating for the temperature rise during the stroke. The first of those is where the butt sits, together with die performance, inspection on the runout table, hot saw length, the finish cut size and the handling system.
The practical instruction attached to it is to check the recovery percentage at the beginning of each die run, not at the end of the month. A die that has started to deflect more, or a butt setting that no longer matches the container, shows up as a recovery figure before it shows up as a customer complaint — and the recovery figure is the only one of the two that costs nothing to read.
Where this leaves a die steel order
Die deflection is a steel property as much as a press property. The die material is chromium hot work steel, AISI H13 and its European equivalent 1.2344, and what holds the opening against the bowing is its hot hardness at the temperature it actually reaches — the working hardness and the temper that gets there are on the H13 tool steel page. The ESR programme for extrusion tooling, which is what a shop buying die steel for thin-wall work should be asking about, is on the 1.2344 ESR H13 supply page; the comparison across the range is on the best tool steels for extrusion dies page.
Around the butt, the pages that carry the rest of the argument are the die bearing length page for the land that sets exit temperature, the die types and tooling page for feeder plates and hollow dies, the die wear page for what a long run does to the land, the tool steel nitriding page for the surface treatment that follows a correction, and the extrusion temperature page for the window the whole calculation runs inside.
Before you set a butt from this page
The published butt percentages are for critical sections and they are guidance, not a schedule. The right butt is set per die, per alloy and per container, and it moves when the liner wears or the die is replaced. Run the etch test on the back end before trusting a thinner butt, and read the recovery figure at the start of every die run. A butt that produces a sound back end at the lowest recovery is the one to keep.
Source, Aluminum Extrusion Technology, P. K. Saha, ASM International, 2000, chapter 6, butt thickness control and productivity control, pages 162 to 165 and 170 to 172.