Tool Steel Hot Hardness Chart

Hot hardness — Rockwell C hardness measured at elevated temperature — for selected high-speed and die steels. The table shows how hardness falls as testing temperature rises, ranking each grade for red hardness in hot-work and high-speed service.

AISIRoom temperature315 °C (600 °F)425 °C (800 °F)540 °C (1000 °F)650 °C (1200 °F)
High-speed tool steels
M16561585432
M26562595536
M3, class 16563605636
M3, class 26563605636
M46663605637
M76561585435
M106560575233
M306563585535
M336564605740
M366564605740
M426866656244
M5064595752—
M5264605753—
T16561575333
T46561595538
T56662605640
T156864615742
Cold-work die steels
A260524635—
A858555245—
D260534738—
D462524637—
Hot-work die steels
H115449474222
H125449474222
H135549474222
H195451474231
H215452494529
H234132302825
H265854504631
  • (a) Small-diameter bars tested according to the recommended heat treatment.

Table notes

Hot hardness measures hardness at elevated temperature after exposure to that temperature — it is the property behind “red hardness” in high-speed and hot-work tool steels. The 540 °C (1000 °F) and 650 °C (1200 °F) columns rank the grades for hot-work service.

The source table lists A8 at the head of both the cold-work and the hot-work groups; it is shown once here, under cold-work die steels.

Values are comparative hardness test results from the source’s reference 7; small variations between heats and test conditions are normal. Reference data for comparison — verify with the applicable heat-treatment schedule for your part.

Related reference pages

H13 tool steel · H11 tool steel · H10 tool steel · H21 tool steel · Hot-work tool steels · Tool steel hardening and tempering chart · Tool steel heat treatment guide · Tool steel properties chart · Tool steel composition chart · How to select tool steels

Source: ASM Handbook, Volume 1 — Properties and Selection: Irons, Steels, and High-Performance Alloys, Table 14 “Hot hardness of selected high-speed tool steels and die steels” (10th ed.). Reference data for comparison — verify the applicable heat treatment before service.