What a Vacuum Furnace Holds, Dew Point and Alloy Depletion in Tool Steel
A vacuum furnace is not an empty furnace, and treating it as one is where tool steel jobs go wrong. The chamber holds a residual gas at a pressure you can measure, that gas has a water content and therefore a dew point, and at the pressures used for tool steel it is thin enough that the alloying elements with the highest vapour pressure leave the surface of the part while it sits at temperature. Chromium and iron go, tungsten and molybdenum stay and their share of the surface rises. This page sets out the dew point each vacuum level actually reaches, why pumping cannot dissociate the oxides, the vacuum each material class needs, and the surface composition change of a high speed steel held at temperature under vacuum.
A vacuum is a gas atmosphere, and it has a dew point
The water vapour that is left in a chamber is the same water vapour that oxidises a steel surface in a gas atmosphere, so a vacuum can be rated by the dew point it reaches in the same way. The source gives two tables for this. The first states the dew point at four vacuum levels on the assumption that the residual gas is 70% water vapour, which is the figure the reference work it draws on uses. The second sets the same calculation out against the water vapour content, so the dew point can be read for a chamber whose residual gas is drier or wetter than that assumption.
| Vacuum, torr | 10-1 | 10-2 | 10-3 | 10-4 |
|---|---|---|---|---|
| -40 | -61 | -76 | -90 |
Dew point of the residual gas at four vacuum levels, assuming the residual gas contains 70% water vapour. Read across to see how much dryness each decade of pressure buys.
| Vacuum, torr | 20% water vapour | 70% water vapour | 100% water vapour |
|---|---|---|---|
| 1 | -35 | -21 | -17 |
| 10-1 | -55 | -43 | -40 |
| 10-2 | -70 | -61 | -58 |
| 10-3 | -86 | -77 | -74 |
| 10-4 | -92 | -90 | -89 |
Dew point as a function of water vapour content at five vacuum levels. The three columns run from a dry residual gas to one that is entirely water vapour, and the spread between them narrows as the pressure falls.
Two figures from these tables are worth carrying into a specification. At 10-1 torr the dew point lies between −40 and −55 °C depending on the water vapour content, and this is the pressure range that is sufficient for hardening tool steels. At 10-2 to 10-3 torr the source states that there is practically nothing left in the chamber that could react with the steel. The source also records the direct comparison against protective atmospheres on high alloy tool steel, where the dew point in vacuum runs between 0 and 18 °C and a vacuum of 5 x 10-1 torr already gives results at least as good as any protective atmosphere.
Why the oxides cannot be dissociated by pumping
It is tempting to assume that a vacuum works by pulling the oxide layer apart, and the source is explicit that it does not. Every metal oxide has a dissociation pressure, and below that pressure the oxide breaks down into metal and oxygen. The dissociation pressure of ferrous oxide, wustite, is around 10-12 torr at 1000 °C and above, which is several orders of magnitude below anything a heat treatment vacuum furnace produces. At the 10-2 to 10-4 torr that a shop actually runs, neither ferrous oxide nor any other oxide dissociates. The dissociation pressures of the metallic oxides, iron oxide among them, are so low that vacuum techniques cannot reach them.
What the vacuum does instead is remove the gases that would form the oxide in the first place, so there is nothing for the surface to react with. That distinction explains a fact that otherwise looks like a contradiction. At 10-4 to 10-5 torr some oxide formation still occurs, and what forms is a semi-transparent film rather than a scale. The film is influenced by the carbon content of the steel, because carbon in the surface reacts with the metallic oxide to form carbon monoxide, which the pumps then remove and exhaust from the chamber.
The vacuum each material class needs
Because the required dryness differs by material, the source gives the working pressure by material class rather than by process. Copper is happy at a rough vacuum, alloyed tool steel and high speed steel harden at 10-1 to 10-2 torr, and the refractory metals need pressures two to six decades lower for the same protection.
| Material to be heat treated | Vacuum, torr |
|---|---|
| Copper | 1 to 10-1 |
| Nickel | 10-1 |
| Alloyed tool steel and high speed steel | 10-1 to 10-2 |
| Heat resistant steel | 10-3 to 10-2 |
| Molybdenum, tungsten | 10-4 |
| Niobium, tantalum | 10-5 |
| Beryllium | 10-7 |
| Stainless steel | 10-3 to 10-5 |
Degree of vacuum required for the heat treatment of various materials. The tool steel and high speed steel row is the one that matters for a tool room order, and it is two to four decades away from the stainless and refractory rows.
The selection advice in the source is a cost argument rather than a purity argument. There is no reason to install a pump system capable of 10-2 torr when the surface quality required is already achieved at 10-1 torr, and the choice of furnace should be settled on the pressure first because it partly fixes the quality reachable and partly fixes the price. The aerospace materials the source mentions, which have to be examined under 10-15 to 10-18 torr, are the far end of that ladder and are not a heat treatment requirement.
Vacuum dew point and alloy depletion in tool steel, printable PDF
The dew point that each vacuum level actually reaches, the vacuum each material class needs, the iron, chromium, tungsten and molybdenum content of a high speed steel surface before and after a vacuum treatment, and the leak test that proves the chamber is holding pressure, in one reference sheet with our contact details.
The alloying elements that leave the surface
This is the effect that makes the vacuum level a process variable rather than a setting. Alloying elements evaporate from a surface at a rate set by their own vapour pressure, and under vacuum the elements with the higher vapour pressure leave preferentially. The source states the effect plainly. Chromium and iron decrease in the surface while molybdenum and tungsten increase, the change grows with the time and the temperature of the treatment, and some alloying elements evaporate excessively under vacuum.
The two tables below come from the same experiment. The composition table gives the two steels that were examined, and the second gives the surface composition of the high speed steel before and after being held at 1000 °C under 10-4 torr. Chromium, the element that carries the wear resistance and the hardenability of the grade, falls from 4.3% to roughly 1.5% in the surface. Iron falls from about 77.5% to about 60%. Tungsten and molybdenum both rise, because as chromium and iron leave, their own share of what remains goes up.
| Material quality | C | W | Mo | Cr | V | Co |
|---|---|---|---|---|---|---|
| High speed steel | 0.8 | 6.0 | 5.0 | 4.3 | 2.0 | 4.75 |
| Chromium steel | 0.48 | 1.6 | – | 1.0 | – | – |
Composition of the chromium and high speed steels examined in the vacuum surface study, in per cent. The high speed steel is the higher alloyed of the two and it is the one the surface figures below belong to.
| Element | Surface content at the start, % | Surface content after the hold, % | Direction of change |
|---|---|---|---|
| Chromium | 4.3 | about 1.5 | falls |
| Iron | about 77.5 | about 60 | falls |
| Tungsten | 6.0 | about 11 | rises |
| Molybdenum | 5.0 | about 10.5 | rises |
Surface composition of the high speed steel of the table above, held at 1000 °C under 10-4 torr. The start values are the analysis of the steel, and the values after the hold are read from the source figure and are therefore approximate. Chromium and iron leave the surface while tungsten and molybdenum concentrate in it.
The same experiment run on the chromium steel, under the same pressure and at three temperatures, shows the same pattern with the magnitude set by the temperature. The practical consequence for a tool steel cycle is that a low pressure is not free. Pumping harder protects the surface from oxidation and at the same time strips the alloying elements out of it, and once the chromium is gone from the surface layer, the hardness and the wear resistance of that layer are gone with it. The evaporated metal also has to go somewhere, and it deposits on the cold parts of the chamber.
Decarburisation, and why it matters less on a tool steel
The source makes a distinction that is easy to miss. A case-hardening steel of more than 0.25% carbon decarburises after only some minutes in the austenitic state under vacuum, because the carbon reacts with the metallic oxide to form carbon monoxide and is exhausted continuously. In a steel of greater carbon content the same effect is observed only after the steel has been heated for four to five hours in the austenitic state. Since a eutectoid or hypereutectoid tool steel does not need a hold of that length, the source concludes that decarburisation is of no importance for it under vacuum. The alloying elements leaving the surface are the real risk, and they are a different mechanism.
One material note belongs with it. Nickel and tungsten resist oxidation by the atomic oxygen that comes from the slow dissociation of carbon dioxide and water vapour better than manganese, chromium or molybdenum do, and steel sits between the two groups. For that reason a chromium or a manganese steel needs a drier or a carbon dioxide lean atmosphere than the rest.
Checking that the chamber is really holding vacuum
Because the whole protection depends on the pressure inside the chamber, the source gives a test that separates the two reasons a furnace will not reach its rated pressure. Pump the chamber to its lowest attainable pressure, and if it does not reach the manufacturer figure that is itself an indication of a leak or of contamination. Then isolate the chamber from the pumping system and watch the rate at which the pressure builds up. A steady rate is a genuine leak. A rate that approaches a limiting pressure and slows as it goes is outgassing or a virtual leak rather than a hole. Only after that is leak detection worth running, and the chamber should be kept clean because the deposits that collect in it are often pyrophoric and can be toxic, and they absorb gas.
Where this leaves a vacuum tool steel order
The three numbers to fix before quoting a vacuum cycle are the pressure, the hold time at temperature, and the temperature itself, because the alloy depletion is driven by time and temperature and only allowed by the pressure. Tool steel hardens at 10-1 to 10-2 torr, and the case to use a lower pressure than that has to be a surface quality the job actually needs. The chromium content of the grade is the guide to how much depletion hurts, because chromium is the element that leaves first and the one a die or a punch is bought for.
The published vacuum cycles for thirteen tool and mould steel grades, with the soak and the cooling gas, are on the vacuum heat treatment page. Which atmosphere a grade is cleared for, and the alloy content thresholds behind that, is on the protective atmosphere selection page, and the chemical effect of the residual gases themselves is on the furnace gas reactions page.
Before you use these values
This page is a reference summary of published practice and it is not an Aobo Steel specification. The dew points, pressures and compositions are reproduced from the source, and the figures read from the source figure are marked as approximate. What a particular furnace produces depends on its pumping system, its leak rate, the load and the cycle. Final selection is confirmed on the job.
Source: Controlled Atmospheres for Heat Treatment, R. Nemenyi and G. H. J. Bennett, Pergamon Press, 1984.