What a Passing Nondestructive Test Report Really Promises
A flaw detection report that returns no rejectable indications is read by most buyers as a statement that the bar is sound. It is not. Every inspection method is quoted against a sensitivity and a probability, and the report is only as strong as those two numbers. This page sets out what a specification actually fixes, how detection is expressed as a probability, and what the published reliability programs found when they measured it.
An inspection is quoted against a sensitivity, not a guarantee
In most industries the inspection requirement is written into a specification, and that specification fixes two things. It fixes the sensitivity level of the method, which is the smallest indication the method has to respond to, and it fixes the size of the flaw that will be rejected. Everything else in the report follows from those two numbers, and a report that does not state them cannot be judged at all.
The published example is an ultrasonic specification for product over 13 mm thick, set on longitudinal wave inspection with flat bottom holes as the reference. It defines five classes of ultrasonic quality, and a class is chosen to suit how critical the part is. Class AA requires that a single discontinuity be detected at a sensitivity equivalent to a No. 3 flat bottom hole, and that multiple discontinuities be detected at the much finer No. 1 level. Class B allows a far coarser No. 8 hole. The full set is as below.
| Quality class | Single discontinuity, flat bottom hole number | Multiple discontinuities, flat bottom hole number | Maximum linear discontinuity, in. | Maximum loss of back reflection, % |
|---|---|---|---|---|
| AA | 3 | 1 | A No. 1 response for 0.12 in. | 50 |
| A1 | 3 | 2 | A No. 2 response for 1.00 in. | 50 |
| A | 5 | 3 | A No. 3 response for 1.00 in. | 50 |
| B | 8 | 5 | A No. 5 response for 1.00 in. | 50 |
| C | As established by purchaser and vendor for the specific part |
Typical NDI acceptance criteria for longitudinal wave inspection of product over 13 mm thick, reproduced from Table 1 of Introduction to Quantitative Nondestructive Evaluation in ASM Handbook, Volume 17. The five quality classes are defined for inspection with flat bottom reflectors in ultrasonic references, and a response is rejected against a loss of back reflection as well as against a hole size. Class C is left to the purchaser and the vendor to agree for the specific part.
The specification then goes on to require three more things before the class means anything. It requires a calibration procedure that demonstrates the system can detect at the stated level, it requires reference blocks made to a published standard so that the demonstration is done against something repeatable, and it requires the personnel to be certified and to work within the limits of their certification.
The flat bottom hole is the yardstick
A flat bottom hole is a flat-ended drilled hole of a known diameter used as the reference reflector, and it was adopted early for a simple reason. It is easy to produce, it is reproducible, it can be made in graduated sizes, it gives a signal similar to a natural imperfection, and it is short enough to resemble the short natural flaws that are hardest to detect. The hole number denotes its diameter as a multiple of 0.4 mm, or 1/64 in., so the numbers in an acceptance table convert to real dimensions as follows.
| Flat bottom hole number | Nominal diameter, mm | Nominal diameter, in. |
|---|---|---|
| No. 1 | 0.4 | 1/64 |
| No. 2 | 0.8 | 2/64, or 1/32 |
| No. 3 | 1.2 | 3/64 |
| No. 5 | 2.0 | 5/64 |
| No. 8 | 3.2 | 8/64, or 1/8 |
Flat bottom hole numbers converted to diameter, from the footing of Table 1 of Introduction to Quantitative Nondestructive Evaluation in ASM Handbook, Volume 17, which states that flat bottom hole numbers indicate diameter in multiples of 0.4 mm, or 1/64 in. A class AA part therefore turns on a single indication no larger than about 1.2 mm across and on multiple indications no larger than about 0.4 mm.
Two footings in that specification are worth carrying into a purchase discussion. A multiple discontinuity is defined as two or more indications above the class level that fall within 1.0 cubic inch, or 16 cubic centimetres, of the inspected surface, which means two small indications close together can reject a part that either one alone would pass. And a partial response is admissible, since 11 percent of a No. 3 flat bottom hole response is treated as equivalent to a No. 1 hole, and 44 percent as equivalent to a No. 2.
Detection is a probability, not a yes or a no
Once detection was measured properly, the question changed from whether a method works to how often it works on a flaw of a given size. The answer is a probability of detection function, and it is described in the volume in these terms. An ideal system would have a probability of detection that is zero below some flaw size and one above it, so that every flaw larger than that size would always be found. No such system exists, and a real probability of detection function is a continuous curve that rises from near zero to near one across a range of flaw sizes.
From that curve comes the single number used to quote a capability, which is the flaw length for which there is a fixed probability that a fixed proportion of flaws of that size will be found. The convention is to choose the length such that, at the 95 percent confidence level, at least 90 percent of all cracks greater than that length will be detected, and the result is written as the 90/95 crack length, with 90 standing for the probability of detection and 95 for the confidence level. Because the confidence level is built in, the same set of test data produces two curves, and the lower one, drawn at 95 percent confidence, is the one a specification is written against.
The confidence level carries most of the weight, and it is the part a buyer usually never sees. A capability quoted at 50 percent confidence is the middle of the measurement, while the same capability quoted at 95 percent confidence is the pessimistic edge of it, and the two can differ by a factor of two in the flaw size they refer to.
The demonstration decides the answer
Because the capability is measured against a set of flawed specimens, the choice of those specimens decides the result. To demonstrate a 90/95 crack size, the specimens in the program have to include cracks smaller than the target size and some larger, and a program built only from large cracks cannot demonstrate a fine capability no matter how well it is run.
The published case study makes the point sharply. Two programs were run on the same requirement of a 90/95 crack depth of 250 micrometres or less, and both were assumed to have detected every flaw presented. Only the second program, whose specimens included the smaller cracks, could demonstrate the requirement at all. The first program, built from larger specimens, returned a 90/95 crack size of 417 micrometres, or 16.40 mils, which is nearly twice the requirement it was trying to prove. The same all-detected result produced two very different conclusions, and the difference lay entirely in how the demonstration was built.
The number of observations matters as much as their sizes. In the B-1 aircraft program the reliability criterion was set at a 90 percent probability of detection with a 95 percent confidence level, and the criterion was met for the largest flaw size in a range only if the inspector missed no more than the following number of the flawed specimens presented.
| Number of observations | Misses allowed to hold 90 percent detection at the 95 percent confidence level |
|---|---|
| 29 | 0 |
| 46 | 1 |
| 61 | 2 |
| 75 | 3 |
| 89 | 4 |
| 103 | 5 |
Detection requirements used to meet a 90 percent probability of detection at the 95 percent confidence level in the B-1 program, reproduced from the reliability data analysis in ASM Handbook, Volume 17. For every flawed specimen presented to an inspector, at least two unflawed specimens were also included in the set.
What the measurement programs actually found
The first large measured program was run in the aerospace industry in the 1970s under the name Have Cracks, Will Travel, and its purpose was to test whether airframe inspection would repeatedly find cracks. It concluded that the overall reliability of the inspection performed by the average technician fell below what had until then been assumed, and that the 90/95 reliability criterion could not be attained for any flaw size with the typical techniques of the day. That result, more than any other, moved the field from assuming a detection capability to measuring one.
Later programs on the same standard produced the numbers below, each quoted at a 90 percent probability of detection and a 95 percent confidence level. They are worth reading against the flat bottom hole table above, because a capability of 0.13 mm on a critical engine part is far finer than a class AA acceptance level on ordinary product.
| Inspection | Demonstrated 90/95 capability |
|---|---|
| Depot eddy current facility for critical engine parts | 0.13 mm (0.005 in.) deep flaws at 90 percent probability of detection and 95 percent confidence |
| Automated retirement-for-cause inspection station, rivet holes | A 100 micrometre (4 mil) crack depth at 90 percent probability of detection and 95 percent confidence |
| Same station, bolt holes and flat surfaces | Reliable detection in the 125 to 250 micrometre (5 to 10 mil) depth range |
| B-1 program production inspection of corner cracks | A 1.3 mm (0.050 in.) depth requirement was not met until the processes were refined and the documentation rewritten |
Reliability demonstrated at a 90 percent probability of detection and a 95 percent confidence level in published aircraft engine and depot inspection programs, reproduced from the NDE reliability and applications articles in ASM Handbook, Volume 17. In the B-1 program the original production processes could not meet a 1.3 mm depth requirement for corner cracks, not all inspection personnel could reach the required reliability even after the procedures were refined, and etching was needed ahead of penetrant inspection before the requirement was met for any of the materials tested.
One further lesson from those programs travels directly to a purchase discussion. The reliability of an inspection is bounded by the qualification of the person running it, and the B-1 program had to turn its demonstration into a formal personnel qualification requirement before a fracture-critical part could be released against it. A method quoted at 90/95 in a specification means nothing unless the shop that runs it has demonstrated that level on that part.
Probability of detection in nondestructive testing, printable PDF
The acceptance criteria classes, the flat bottom hole yardstick, the demonstration statistics and the 90/95 capability demonstrated in service, in one PDF with our contact details.
Grades and stock
The acceptance numbers in a report are only meaningful next to the method that produced them, and the methods are set out on the page on choosing a nondestructive test method. How those methods behave on bar and billet, including the seam depth a permeability system reaches and the blind length at each end of a bar, is on the bar and billet inspection page.
Where a report comes with a certificate, the two documents answer different questions, and the certificate side is collected on the steel bar and billet inspection page. The mechanical test that most often sits beside a flaw detection report on a tool steel order is the impact test, described on the Charpy impact test page, and the surface defects a report is checking for are catalogued on the steel bar defects page.
Probability of detection in nondestructive testing, printable PDF
The acceptance criteria classes, the flat bottom hole yardstick, the demonstration statistics and the 90/95 capability demonstrated in service, in one PDF with our contact details.
Before you use these values
This page is a reference summary of published practice and it is not an Aobo Steel specification. The acceptance classes, the flat bottom hole conversions and the reliability figures are reproduced from the source, and every one of them applies to the part, the method and the calibration it was measured on. A capability claimed for one part does not transfer to another without a demonstration.