H13 Tool Steel Hardness

H13 tool steel hardness ranges from about 220–241 HB in the annealed condition to 51–54 HRC after quenching, with finished tools typically tempered to 38–55 HRC. Most hot-work tooling runs around 40–48 HRC. The exact target depends on section size, heat treatment, and the application the tool is built for.

Supplied H13 is normally annealed for machining at around 220–241 HB. After quenching, standard sections reach about 51–54 HRC, while large sections can show lower core hardness because the center cools more slowly than the surface.

After tempering, finished H13 tools are commonly adjusted within about 38–55 HRC. Many hot-work tools work around 40–48 HRC, with lower hardness often used for heavy shock and higher hardness used where wear resistance is more important.

Final hardness can change with section size, austenitizing temperature, cooling rate, tempering practice, and test position. For most H13 tooling, the target is balanced hardness, not maximum hardness.

Aobo Steel supplies H13 tool steel in an annealed condition for bulk orders, including round bar, flat bar, plate, and forged block. For purchase, see the H13 product page or contact [email protected]

H13 Tempering Temperature and Hardness Chart

Tempering adjusts quenched H13 to its final usable hardness. It reduces brittleness, relieves internal stress, stabilizes the microstructure, and improves service reliability.

H13 is commonly austenitized at about 995–1025°C (1825–1875°F) before quenching. After quenching, it is usually double-tempered or triple-tempered to improve stability and reduce the risk of brittle failure.

Tempering TemperatureApproximate Hardness
As quenchedAbout 51–54 HRC
400–600°F / 204–316°CAbout 51–53 HRC
950°F / 510°CAbout 52–54 HRC
980°F / 527°CAbout 52 HRC
1030°F / 555°CAbout 50 HRC
1050°F / 566°CAbout 44–46 HRC
1065°F / 575°CAbout 48 HRC
1100°F / 593°CAbout 41–46 HRC
1120°F / 605°CAbout 44 HRC
1150°F / 621°CAbout 36–38 HRC

Some values overlap because different reference data may use different austenitizing temperatures, quenching methods, holding times, section sizes, and test positions. These values should be used as H13 heat-treatment guidance.

For hot-work tooling, the highest HRC value is not always the best target. A slightly lower but more stable hardness can often give better tool life when the tool faces impact, thermal cycling, or large-section stress.

The optimal hardness for H13 depends on how the tool operates and how it is likely to fail. Die casting, forging, extrusion, and high-shock tooling place different demands on the steel.

ApplicationTypical H13 Working HardnessSelection Logic
General hot-work toolingAbout 40–48 HRCBalanced hot strength, toughness, and wear resistance
Aluminum and magnesium die casting diesAbout 42–52 HRCDepends on die size, thermal cycling, and wear demand
Common die casting inserts and coresAbout 44–48 HRCBalanced heat-checking resistance and wear resistance
Zinc die casting diesAbout 50–52 HRCLower casting temperature may allow higher hardness
Hammer forging diesAbout 40–47 HRCLower hardness improves shock resistance
Press forging diesAbout 47–55 HRCLess sudden impact allows higher hardness
High-shock toolingAbout 40–44 HRCToughness is more important than wear resistance
Aluminum and magnesium extrusion diesAbout 42–45 HRCBalance of hot strength and cracking resistance
Copper and brass extrusion diesAbout 42–48 HRCHigher thermal and pressure demand
Steel extrusion diesAbout 47–51 HRCHigher hot strength and wear resistance required
MandrelsAbout 46–52 HRCHigh-temperature strength and wear resistance are required
Dummy blocks and ramsAbout 40–44 HRCToughness and heat resistance are important
Extrusion containersAbout 35–40 HRCLower hardness improves toughness in large sections

For die casting dies, hardness must be balanced against heat checking. Large inserts are often kept at a lower hardness to reduce the risk of cracking, while smaller inserts can be made harder when wear resistance is more important.

For forging dies, impact severity is the main concern. Hammer forging normally requires lower hardness than press forging because the loading is more sudden and severe. If hardness is pushed too high, the die may crack before wear becomes the main problem.

For extrusion tooling, the tool function matters. Dies, mandrels, dummy blocks, rams, liners, and containers should not automatically be assigned the same hardness, as they experience different thermal and mechanical loads.

A simple selection rule is that when wear and plastic deformation dominate, a higher working hardness may help. When cracking, chipping, severe impact, or thermal fatigue dominate, a lower or more balanced hardness is usually safer.

FAQ

What is the typical hardness of H13 steel?

The hardness of H13 steel depends on its condition and heat treatment. In the annealed condition, H13 is usually around 220–241 HB. After hardening and tempering, finished H13 tools are commonly adjusted within about 38–55 HRC, with many hot-work tools used around 40–48 HRC.

What is the annealed hardness of H13 steel?

The annealed hardness of H13 steel is usually around 220–241 HB. This is the common soft condition for machining before final hardening and tempering.

What is the hardness of H13 after quenching?

After quenching, standard H13 sections may reach about 51–54 HRC. Large sections can show lower core hardness because the center cools more slowly than the surface.

What is the typical working hardness of H13 tool steel?

Many H13 hot-work tools work around 40–48 HRC. The exact working hardness depends on tool size, operating temperature, impact load, wear demand, and failure risk.

What hardness is used for H13 die casting dies?

H13 die-casting dies are often used at 42–52 HRC. Common die casting inserts and cores are frequently selected around 44–48 HRC, depending on die size, thermal cycling, and wear conditions.

What hardness is used for H13 forging dies?

H13 hammer-forging dies are often used at around 40–47 HRC because the impact severity is high. Press forging dies may use a higher range, often around 47–55 HRC, because the loading is less sudden.

What hardness is used for H13 extrusion dies?

H13 extrusion dies are commonly selected according to the extruded material. Aluminum and magnesium extrusion dies are often around 42–45 HRC, copper and brass extrusion dies around 42–48 HRC, and steel extrusion dies around 47–51 HRC.

Is higher H13 hardness always better?

No. Higher hardness can improve wear resistance and resistance to plastic deformation, but it can also increase the risk of cracking, chipping, and heat checking. For H13 tooling, hardness should be selected according to the main failure mode.

Why do H13 hardness values overlap in tempering charts?

H13 tempering hardness values can overlap because results depend on austenitizing temperature, quenching method, holding time, section size, tempering practice, and test position. Tempering charts should be used as guidance, not as guaranteed hardness values for every tool.