Brazing Tool Steels

Brazing joins tool steel at a temperature below the melting point of the steel, which makes it a way to set an insert into a die body or to attach a wear pad without putting the whole tool through a welding procedure. The window is narrower than it is on plain carbon steel. A tool steel is tempered martensite carrying a fine dispersion of carbides, and that structure reacts badly to uneven heating. This page covers the filler metal groups, the brazing processes, the atmospheres and fluxes, and the way a braze can be built into the hardening cycle instead of run before it.

Why tool steel is harder to braze than plain carbon steel

Tool steels are high-alloy steels built for high hardness and wear resistance, and they split into two working groups. In carbon tool steels the mechanical properties come mainly from the carbon content, which runs between 0.6 and 1.4 wt%. In high speed tool steels the carbon is generally lower and the properties come from the alloying elements, tungsten, molybdenum, chromium and vanadium. All four of those are carbide formers. The carbides change how a molten braze alloy wets and spreads at the microstructural level, and they also change the character of the iron oxide on the surface, which makes wetting and spreading more difficult than it is on a plain carbon steel.

The second problem is the structure itself. A tool steel has higher hardenability than a low-carbon or low-alloy steel, and its usual condition is tempered martensite with a fine dispersion of carbides, a structure that is sensitive to thermal gradients and can crack under them. During cooling the outer part of a component transforms to martensite and expands, while the core is still hot and untransformed. That difference in phase, on top of the difference in thermal expansion, builds residual stress and can crack the transition zone between the transformed and untransformed metal. The heating and cooling of a tool steel braze therefore has to be controlled closely enough to keep the gradient through the part small.

Filler metals for tool steel

The silver, copper and nickel brazing filler metal groups all work on tool steel, and which one is chosen depends on the application, the equipment on hand and the strength the joint needs. Silver based filler metals suit torch and induction brazing. Copper and nickel based filler metals are furnace products. Their working ranges are wide apart, with the copper based group brazing between 1095 and 1150 °C (2000 to 2100 °F), the copper-zinc group between 910 and 982 °C (1670 to 1800 °F), and the silver based group between 620 and 900 °C (1145 to 1650 °F). Where the joint only has to serve at moderate temperature, copper based filler metals below 480 °C (900 °F) and silver based filler metals below 425 and 200 °C (800 and 400 °F) have a long record of successful use. The filler metal groups used on tool steel are the same ones used on low-carbon and low-alloy steel, with one qualification. Some tool steels carry a higher chromium content than those steels do, and the flux has to be designed to promote wetting despite the oxidation potential of chromium.

Brazing inside the hardening cycle

Because the brazing temperature of the copper based group sits above the austenitizing temperature of many steels, a braze can be run as the first step of the heat treatment rather than before it. The two routes follow the filler metal. Where the brazing temperature is higher than the A1 temperature of the steel, the braze is made during the austenitizing part of the cycle. Where the brazing temperature is lower, the braze is made alongside the first or the secondary tempering step instead. A high solidus filler metal is what makes the first route possible, because the joint has to survive the quench without remelting.

The worked example in the source is a plate assembly in 4340. It is brazed with copper filler metal at 1120 °C (2050 °F) for 10 minutes, then held at 845 °C (1550 °F) for one hour to austenitize the base metal and quenched in oil. The temper is two hours at 510 °C (950 °F), which brings the part to about 40 HRC. The copper braze is unaffected by that sequence because its melting point sits well above every temperature in it. A tool steel that is brazed and then hardened has to be supplied in a condition that supports the cycle, because a braze run on a part that is already hardened and tempered cannot then be quenched again without losing the dimensions the tool was finished to.

Which brazing process to use

Tool steels can be brazed by most of the brazing processes, and the differences between them matter more here than they do on a low-carbon steel. Furnace brazing gives the tightest control of both temperature and the brazing cycle, and it carries one condition with it. The furnace atmosphere has to be regulated, because the wrong one decarburizes or carburizes the base metal and degrades the steel the joint is holding together.

Torch brazing is the process to be careful with. It gives the operator no accurate control of temperature, and thermal cracking during a torch braze on tool steel is common rather than exceptional. Induction brazing can be used, provided a ductile metal insert is placed in the joint. The soft metal absorbs part of the residual stress that the braze generates and lowers the tendency to crack. A composite filler metal, a copper-silver-copper sandwich, does the same job in a different way by balancing the shear stresses that build up across the joint as it cools.

Atmospheres, fluxes and cleaning

Low-alloy steels and tool steels can be brazed in air, in vacuum, in hydrogen or nitrogen, or in endothermic and exothermic atmospheres. Components brazed with nickel based filler metals are usually run in vacuum, while vacuum, nitrogen and hydrogen are the usual choices for copper based and silver based filler metals. Whatever atmosphere is chosen has to be checked against the decarburization and carburization risk to the steel.

Cleaning follows the condition of the part. A freshly machined component normally needs only a vapour degrease or a solvent wipe to take off machining lubricants. A component with a light oxide layer can be grit blasted with aluminium oxide and then vapour degreased, or rubbed back with emery paper or a stainless steel wire brush and wiped with solvent. A heavy oxide layer needs mechanical and chemical cleaning together. Vacuum or hydrogen furnace cleaning is a further option. It reduces the oxides of iron and nickel, and it does not necessarily reduce the other oxides on the surface.

Flux selection runs against the chemistry of the steel. Surface oxides are what hold a braze back, and on a low-carbon or low-alloy steel they come off easily enough with a flux or an atmosphere. Chromium changes that. Above about 1.0 wt% chromium, and where aluminium or titanium is present, the oxide becomes harder to remove, because those elements make the oxide adhere more firmly and slow the diffusion of oxygen through it. The flux or the brazing atmosphere has to be able to reduce that oxide and promote wetting, and the recommended brazing conditions differ between steels above and below the 1.0 wt% chromium line. Fixturing on tool steel brazements can lean more on metal fixtures than a high-temperature braze allows, because many of these joints are made at lower temperatures. Soft soldering of tool steel is not a common practice, simply because there are few applications for it.

Where brazing fits on a tool

Brazing earns its place on the joints a die or a mold has to make without disturbing the body. Setting a carbide or a harder alloy insert into a die, attaching a wear pad to a surface that will not be rebuilt by welding, and joining a tool body from several pieces before final machining are the usual cases. All of them are easier when the steel is ordered annealed and the braze is planned into the hardening cycle rather than added on after it, because that is what keeps the dimensions and the hardness of the finished tool under control.

Source: ASM Handbook, Volume 6, Welding, Brazing and Soldering, ASM International, 1993.