Casting the Billet: Pouring Temperature, Casting Speed and the Defects Between Them
Every billet that reaches a press has already been through a narrow window once. In direct chill casting, molten metal freezes in a water-cooled mold while the bottom of the mold descends, and the casting speed decides whether the shell is thick enough to hold the liquid inside it. Cast too slowly and the surface wrinkles; cast too fast and the shell is remelted from within, or the thermal stress from skin to centre exceeds what the alloy can take and the log splits. Everything else in the casting house — gas removal, filtration, grain refinement, homogenization — exists to make that window wider and the metal inside it cleaner. This page is the casting side: the variables, the numbers, and what each defect looks like on the log.
What those billet properties then do at the press — the segregation layer, gas, inclusions and the Mg2Si state seen as pick-up, streaks and blisters — is on the billet quality page. This page stays in the cast house.
The five variables the cast house actually controls
| Variable | Published setting | What it controls |
|---|---|---|
| Pouring temperature | 28 °C above the alloy liquidus at the casting unit | Gas pickup and oxide formation; too hot and both rise |
| Casting speed | For 6063: 130 mm/min at 178 mm diameter, 100 mm/min at 230 mm | Shell thickness, sump depth, cold shuts against bleeding and cracks |
| Mold type | 6061 and 5052 are suitable mold alloys; hot-top and air-bearing molds dominate | Heat extraction through the wall, and therefore the surface and the subsurface |
| Metal head | At least 51 mm from mold bottom to metal surface | The pressure that feeds the mold and holds the freeze line |
| Water flow | About 1 MJ of heat removed per kg of ingot; water must wet the whole surface and cascade | Cooling rate; water that bounces off cools nothing |
Casting variables and the published values for them. Pouring temperature is quoted at the casting unit, not in the furnace, because the metal cools on the way.
The pouring temperature is usually described as a single offset, but it is set per alloy system because the liquidus moves with the alloy:
| Alloy system | Liquidus, °C | Casting temperature, °C |
|---|---|---|
| Al, AlMn | 660 | 688 |
| AlMg, AlMgSi | 650 | 680 |
| AlCuMg, AlZnMgCu | 640 | 670 |
Liquidus and casting temperatures by alloy system. The offset is the same 28 °C in all three rows; the absolute temperature is not.
Hydrogen is the only gas that matters
Hydrogen is the only gas appreciably soluble in aluminum, at about 1.4 ppm in the liquid and about 0.12 ppm in the solid. That ten-to-one drop across the freezing front is the whole problem: what the liquid can hold, the solid cannot, and the difference comes out as porosity in the casting and as blisters later in the extrusion and in the heat treatment of hard-alloy shapes. Sources are the furnace atmosphere, the charge, the fluxes, the refractory components and metal-to-mold reactions.
Degassing is done in-line, between the holding furnace and the casting machine, and the published performance figures are worth having in mind when a supplier describes their unit: in-line gas fluxing removes 61 to 66% of the hydrogen and better than 65% of the inclusions, and independent modelling of a cylindrical-rotor fluxing unit confirmed 61% hydrogen and 67% particulate removal. Rotary systems such as SNIF distribute the fluxing gas as fine bubbles through a spinning nozzle, using argon or an argon-chlorine mixture; chlorine is the most efficient degassing gas for aluminum, and the reason it is not used freely is that the chlorination step needs a strict exhaust processing system.
Filtration follows, on-line, immediately before the mold. The published description of it is blunt — filtration is the heart of billet quality — and the inclusions it is there to catch are specific: oxides such as Al2O3 and MgO, spinels such as Mg2AlO4, borides, carbides, nitrides, refractory fragments, and intermetallics that are wanted in fine distribution but counted as inclusions when they appear as large primary phases. Ceramic foam filters, in commercial use since 1974, work as deep-bed filters: most of what they retain is smaller than the pore opening and is trapped through the depth of the structure rather than screened out at the face.
Grain refinement: what the titanium-boron addition buys
The target structure is fine and equiaxed, and the classic demonstration is a set of 7016 billets cast with and without a titanium grain refiner. Without it the structure is coarse and feathered; with it, fine and equiaxed. A band of large grains remains at the surface regardless of mold type, and because the depth of liquation varies inside that band, the actual liquated zone is hard to measure precisely.
What the refiner buys is both a casting and an extrusion result. In casting it minimizes shrinkage, hot cracking and hydrogen porosity. In the extrusion it improves mechanical properties, the response to thermal treatment, the appearance after chemical or electrochemical finishing, and the resistance to surface tearing. The standard refiners are titanium-boron master alloys.
The casting window: too slow and too fast are both defects
This is the part of casting that a press shop usually meets only as a scrap statistic. The published instruction is a compromise in one sentence: the billet must be cast fast enough to avoid cold shutting, and slowly enough to avoid splitting, bleeding and liquation.
| Defect | What it is | Casting cause | Direction of the fix |
|---|---|---|---|
| Centre crack or split | Internal thermal stress cracking, worst in AlCuMg and AlZnMgCu, sometimes AlMgSi | Contraction difference from skin to centre as the shell freezes first | Slower casting, lower temperature |
| Bleeding | Molten metal running down the already-solidified surface | Remelting through a thin shell under hot centre metal | Slower casting |
| Cold shut | A wrinkle on the surface, 3.2 to 6.4 mm deep | Slow casting followed by rapid cooling | Faster casting |
| Liquation | Low-melting constituents oozing to the outside surface | Same mechanism as inverse segregation, plus freezing and partial remelting against the cold mold | Mold and cooling practice, not speed alone |
The casting window has a defect on each side. The four defects above explain why a casting speed cannot be optimized on surface appearance alone.
Surface quality is governed by the shape of the sump — the liquid pool in the head of the billet. Its depth is set by casting speed, cooling condition and mold system, which is another way of saying it is set by the heat transfer during solidification, and it grows as casting speed rises. In the published horizontal casting work on 6063, good surface finish was obtained when the sump depth was half the billet diameter.
The segregation band, in numbers
Inverse segregation puts the low-melting, solute-rich metal at the outside of the billet, and the mechanism is shrinkage: aluminum alloys shrink about 6% on solidifying, and the liquid at the centre is pushed outward to fill the gaps left in the already-solidified skin. The band is present to some degree on practically every extrusion billet, normally 100 to 200 µm deep, and it carries coarse iron-rich intermetallic and can be rich in magnesium and silicon. That is the layer an anodized part shows as a streak and the layer a scalping operation removes.
Mold technology moves the number. Air-bearing molds — the AirSlip type introduced in 1983, with a short mold and a permeable graphite ring that holds a gas-and-oil film between metal and mold — restrict the inverse segregation zone to about 1 mm for all alloys cast, and give a shallow liquation zone that needs less scalping on an indirect extrusion billet. Alloys from 1100 to 7150 are cast this way commercially.
Scalping itself is the machining of the liquated skin. It is standard for hard alloys, and for wide soft-alloy sections where the circumscribing circle of the die comes close to the container bore. For hard alloys, and especially for indirect extrusion where there is no relative movement between billet and container to redistribute the skin, machined billets are the recommendation — their skin is much harder than that of a soft alloy, and it does not wash off.
Homogenization: three steps, one temperature ceiling
As-cast billets are usually homogenized before extrusion, and the published list of reasons is a list of what the press would otherwise absorb: grain-boundary and dendritic cell segregation with low-melting eutectics and brittle intermetallics that reduce workability; supersaturated precipitates such as Al6Mn, AlFeMn and Mg2Si that raise high-temperature flow stress; manganese, iron and zirconium that retard recrystallization; Mg2Si already precipitated during cooling after casting, which reduces the hardenability of the extruded section and spoils bright-finish work; and grain-boundary segregation that shows as a streaked texture after anodizing.
The cycle is three steps: heat at a controlled rate, hold at temperature, cool at a controlled rate. The controlling physical quantity is the diffusivity of the alloying elements at the hold temperature, so a higher temperature reaches homogeneity faster — and the ceiling is the lowest-melting phase in that alloy. Go above it and the damage is local melting: voids, segregation, blistering and cracking that cannot be repaired afterwards.
| Alloy | Homogenizing temperature, °C | Holding time, h |
|---|---|---|
| 1060 | 560 to 580 | 6 |
| 1100 | 580 to 600 | 6 |
| 2014, 2024 | 480 to 490 | 12 |
| 5052 | 550 to 560 | 12 |
| 5083, 5086 | 520 to 540 | 12 |
| 5454, 5456 | 550 to 560 | 12 |
| 6061 | 560 to 570 | 6 to 8 |
| 6063, 6101, 6463 | 560 to 580 | 6 |
| 7001 | 460 to 480 | 12 |
| 7075, 7079 | 470 to 480 | 12 |
Typical billet homogenizing temperatures and holding times. The hard alloys sit 100 °C lower than the 6xxx grades, which is the solidus ceiling showing through the practice.
Cooling is the third step and it is not a formality. Manganese additions up to 0.027% showed no measurable effect on Mg2Si precipitation in 6063, but the cooling rate does: slow cooling precipitates more Mg2Si and leaves less magnesium in solid solution, fast cooling does the opposite. Quenching after homogenization raises the properties of the billet itself and lowers the properties of the extrusions made from it, compared with air cooling — a billet specification written on billet properties alone can therefore cost the extruder section strength. Continuous homogenizing furnaces, where billets move through on a walking beam in a single layer, give every billet the same time and temperature; a batch furnace does not, and the dispersion between the hot side and the cool side of the load is a real spread in the product.
Where this leaves a die steel order
Nothing in the cast house is bought from a die steel supplier, but everything cast there arrives at the die. The segregation skin is what a bearing sees when a billet is not scalped, the inclusions are what a filter did not catch, and the sump and the grain structure decide how the metal flows when the die is finally loaded. The billet side of that handover is on the billet quality page; the oxide that the skin becomes in the container is on the container liner and dummy block page; the butt that keeps it out of the section is on the butt thickness and yield page.
On the die side, the consequences are the pages that follow: the bearing that takes the wear on the die bearing length page, the wear pattern itself on the die wear page, the grade choice on the best tool steels for extrusion dies page and the H13 tool steel page, and the extrusion grade with its ESR supply on the 1.2344 ESR H13 page.
Before you quote a billet from this page
These are published casting parameters and defect mechanisms, not a cast house schedule. Casting speed, pouring temperature and cooling are set per alloy, per diameter and per mold on that machine, and the window is narrow enough that a change of mold changes all three. Ask a billet supplier for the casting speed, the degassing unit and the homogenizing cycle by alloy — and treat a billet that is only specified by chemistry as unspecified.
Source, Aluminum Extrusion Technology, P. K. Saha, ASM International, 2000, chapter 5, billet casting principles and practice, pages 120 to 145.