Choosing the Press: Specific Pressure, Direct or Indirect, and the Line Behind the Die
A press is bought as a tonnage and used as a pressure. The tonnage is fixed by the hydraulics; the pressure the billet actually sees is that tonnage divided by the area of the container bore, so the same press becomes a different machine when the container is changed. A 2,500 ton press with a 254 mm bore develops 439 MPa of specific pressure; the same press with a 203 mm bore develops 685 MPa. One will extrude a hard alloy at low temperature and the other will not, and neither number appears on the nameplate. This page is about that calculation, the choice between direct and indirect extrusion, and the equipment between the log and the age oven that decides whether the press is ever the bottleneck.
Tonnage is not capacity; specific pressure is
The published selection rule is that the unit pressure required for the extrusion is the principal consideration, and the specific pressure of the press has to exceed it. That is a different statement from “buy enough tonnage”, because raising the container bore lowers the specific pressure at the same tonnage and the extrusion capability falls with it.
| Press capacity | Bore 1 | Bore 2 | Bore 3 |
|---|---|---|---|
| 500 t (5.0 MN) | 76.2 mm — 971 MPa | 101.6 mm — 547 MPa | 127.0 mm — 352 MPa |
| 1,000 t (10.0 MN) | 101.6 mm — 1,089 MPa | 127.0 mm — 703 MPa | 152.4 mm — 487 MPa |
| 1,500 t (15.0 MN) | 152.4 mm — 731 MPa | 177.8 mm — 537 MPa | 203.2 mm — 407 MPa |
| 2,000 t (20.0 MN) | 177.8 mm — 716 MPa | 203.2 mm — 548 MPa | 228.6 mm — 434 MPa |
| 2,500 t (25.0 MN) | 203.2 mm — 685 MPa | 228.6 mm — 542 MPa | 254.0 mm — 439 MPa |
| 3,500 t (35.0 MN) | 228.6 mm — 759 MPa | 254.0 mm — 615 MPa | 279.4 mm — 508 MPa |
| 4,000 t (40.0 MN) | 254.0 mm — 703 MPa | 279.4 mm — 581 MPa | 304.8 mm — 487 MPa |
Standard press capacities, the container bores normally offered with them, and the specific pressure each combination develops. Published values, reproduced for the capacities above; the source lists every capacity from 500 to 4,000 tons.
Two practical readings follow from the table. The first is that container bore, not tonnage, is the number to quote when a customer asks whether a shape is possible: a 3,500 ton press at 279 mm is a weaker machine per square millimetre than a 2,000 ton press at 178 mm. The second is that the required pressure itself is not a constant — it moves with the alloy and its condition, the extrusion ratio, the billet length and temperature, the extrusion speed and the circumscribing circle of the shape. Heavy sections with a large circle go on a high-capacity direct press; small, thin, tight-tolerance work is where the indirect process earns its place.
Direct, indirect, and the friction difference between them
In direct extrusion the billet slides in the container, and that friction is what separates the processes. In indirect extrusion the die sits on the front of a hollow stem that penetrates the container, and there is no relative displacement between billet and container at all. The published consequence is large enough to change the press spec: indirect extrusion allows a twofold increase in billet weight and in extrusion speed, with a 30 to 45% decrease in extrusion force.
| Advantages of indirect | Disadvantages of indirect |
|---|---|
| Longer initial billets | Billet skin must be machined to prevent surface imperfections |
| Higher extrusion speed for many materials | Extrusion size limited by the bore of the hollow stem |
| Thinner butt ends | Die handling is difficult |
| More uniform structure along the length | Smaller circumscribing circle than a direct press of the same rating |
| Thinner sections and closer tolerances over the full length | Higher stress on the stem |
| More uniform container and billet temperature; longer container and liner life | Combination presses give no compensation for the indirect advantage |
The published comparison between direct and indirect extrusion. The scalping requirement is the one that lands on the billet supplier, not the press builder.
Direct extrusion of the hard alloys — 2024 and 7075 named in the source — carries its own list of limits: billet weight, extrusion speed, recovery, productivity, dimensional accuracy, and structural uniformity along the length. That list is the reason a shop running aerospace work thinks about an indirect press at all.
A third process sits between them and is worth knowing by name even though it is rare: extrusion with active friction forces, or active indirect extrusion, in which the container or die moves relative to the ram so that container friction acts in the direction of metal flow instead of against it. In the published figures it extrudes at three to four times the speed of the direct process and two to three times that of the indirect process, with fewer defects and a more uniform structure. It has been in industrial use in Russia since 1988 on presses of 1,600 and 3,500 tons.
Alignment and stiffness: the part of the specification nobody reads twice
Three components have to lie on one centreline for the die to work as designed: the container with its liner, the stem with its dummy pad, and the die slide with the die stack. Modern presses carry a relative position indicator to monitor container and moving crosshead alignment during the stroke, and the machine itself is built as a prestressed tie-rod frame with long die stacks so that deflection under load is small — which is the same deflection that decides whether a thin wall comes out to tolerance.
The reason to buy stiffness rather than tonnage is in the application. A press that deflects closes the die opening at the centre of the section, and no die correction can compensate for a press that changes shape under load.
The container and its liner
The container is the most expensive wearing part on the line and its life is a profitability item, not a maintenance item. The published design criteria are the specific pressure inside the liner, the maximum outside diameter of the container, and — for a rectangular container — the width-to-height ratio. The container is heated to about 427 °C by resistance units in the container or its holder, and large presses use multizone control, six independent zones in the published example, because a wraparound element cannot hold an even temperature along a very long liner. An induction heater in the container can reach about 500 °C.
The liner life figure is worth quoting to anyone who asks why liner steel matters: a liner made of a suitable steel with high resistance to softening, fitted in a correctly designed container, can withstand 30,000 to 40,000 cycles. A rectangular container is used where wide sections are the business — aircraft landing mats are the published example — and it also gives a more uniform metal flow, which lowers the specific press load.
The line behind the die decides the output
The published position is that the performance of an extrusion plant depends largely on its auxiliary equipment, and the productivity block diagram has three systems feeding it: billet heating and length control, the press itself, and the handling system. Each of them controls both downtime and scrap.
| Equipment | What it does to the process |
|---|---|
| Log heater with hot log shear | Shears each log to the billet length a particular die needs; a short billet reduces the breakthrough pressure on the first billet, which protects the die bridges when the die is not yet heat balanced |
| Taper quench or induction shock heater | Creates the front-to-back temperature gradient that makes isothermal extrusion possible |
| Hot billet scalper | Machines the skin for indirect extrusion of aircraft alloys, where the billet does not slide and the skin cannot be redistributed |
| Multichamber die oven | Holds each die at its own temperature; the nitrogen-atmosphere version also prevents high-temperature oxidation and removes the thermal shock of a chest-type oven |
| Die cassette heater | Keeps the die at temperature at the die-change position, and holds the shearing face in position against thermal expansion |
| Water-spray quench on the runout | Replaces tank quench and cooling fans; high-velocity sprays with air-assisted atomization cool difficult shapes below the critical temperature |
| Single or double puller with hot saw | Holds exit speed and tension, and lets the press cut to length without stopping |
| Automatic stretcher, saw and stacker | Straightens, cuts and stacks without handling damage; the published layout puts television cameras on the stretcher and laminated clamping heads at both ends |
Auxiliary equipment on a modern line and the process variable each one owns. The source lists the same items as the equipment of an integrated installation from log heating to age ovens.
The published productivity list is short enough to use as a checklist: the correct billet size at the optimum temperature, using log heating with hot log shear and taper quench; the correct die and tooling temperature to cut avoidable downtime; exit speed and temperature controlled with an automatic double puller; and an automatic handling system from runout to stacking and aging, to cut handling damage and labour.
One detail from the die-change position is worth taking back to the die shop. On a large press the die stack is long, and the shearing face moves with thermal expansion and contraction. When the shearing face is not positioned properly, smeared aluminum appears on the die face, and the next billets flare or blister. That is a die carriage and heater problem with a die-face symptom — the kind of fault that gets blamed on the die steel and is not.
Where this leaves a die steel order
Press selection decides what the die has to take: the specific pressure at the container bore, the deflection of the stack, and how hard the line pushes the exit temperature. Once those are fixed, the die material is the variable left — chromium hot work steel, AISI H13 and its European equivalent 1.2344, in the working hardness and temper set out on the H13 tool steel page, with the extrusion-tooling ESR programme on the 1.2344 ESR H13 supply page.
The rest of the chain: the stack that has to fit the press on the die types and tooling page, the land that sees the pressure first on the die bearing length page, the wear that follows on the die wear page, the nitriding that protects it on the tool steel nitriding page, and the section-and-press limit itself on the circumscribing circle diameter page.
Before you buy or quote a press from this page
Specific pressure is a selection criterion, not a guarantee. The published table assumes the container bores listed, and the required pressure for a real shape still has to be checked against the alloy, the extrusion ratio, the billet length and temperature, the speed and the circumscribing circle. A press that meets the number on paper and deflects under load will not hold the tolerance, and no table in a book can confirm the machine in your bay.
Source, Aluminum Extrusion Technology, P. K. Saha, ASM International, 2000, chapter 3, extrusion press and auxiliary equipment, pages 56 to 85.