Tool Steel Thermal Conductivity Chart

Thermal conductivity versus temperature for seven tool steels — W1, H11, H13, H21, T1, T15 and M2 — in W/m·K and Btu/ft·h·°F, from 95 °C (200 °F) up to 815 °C (1500 °F). Conductivity sets how quickly heat moves through a die or tool: the higher the value, the easier the tool sheds heat to its surroundings.

TypeTemp.
°C
Temp.
°F
W/m·KBtu/ft·h·°F
W19520048.327.9
26050041.524.0
40075038.122.0
540100034.620.0
675125029.417.0
815150024.214.0
H119520042.224.4
26050036.321.0
40075033.419.3
540100031.518.2
675125030.117.4
815150028.616.5
H1321542028.616.5
35066028.416.4
47589028.416.4
605112028.716.6
H219520027.015.6
26050029.817.2
40075029.817.2
540100029.417.0
675125029.116.8
T19520019.911.5
26050021.612.5
40075023.213.4
540100024.714.3
T159520020.912.1
20050024.113.9
40075025.414.7
540100026.315.2
M29520021.312.3
20050023.513.6
40075025.614.8
540100027.015.6
675125028.916.7

Table notes

Thermal conductivity as a function of temperature, in both metric (W/m·K) and imperial (Btu/ft·h·°F) units. The imperial values equal the metric values × 0.578; the temperature sets differ between grades as printed in the source.

Note: for T15 and M2 the second temperature pair is printed as 200 °C / 500 °F. These are not exact conversions of each other (500 °F = 260 °C); the pairs are reproduced as printed.

H13 sits in a narrow band of about 28.4–28.7 W/m·K from 215 to 605 °C, while the tungsten and molybdenum high-speed steels run roughly 20–29 W/m·K depending on temperature — useful when balancing heat removal in die casting, extrusion and forging tooling. Verify against the applicable heat treatment before design use.

Related reference pages

H13 tool steel · H11 tool steel · H21 tool steel · M2 tool steel · Hot-work tool steels · Hot-work tool steel softening resistance · Tool steel density and thermal expansion · Tool steel hot hardness chart · Tool steel properties chart

Source: ASM Handbook, Volume 1 — Properties and Selection: Irons, Steels, and High-Performance Alloys, Table 12 “Thermal conductivity of selected tool steels” (10th ed., pp. 1817–1819). Reference data for comparison — verify the applicable heat treatment before design use.