440C Steel Technical Overview
440C Steel Technical Overview: 440C steel is a high-carbon, high-chromium martensitic stainless steel with a typical composition of 0.95-1.20% Carbon and 16.0-18.0% Chromium. This yields high hardness, reaching approximately Rockwell C 60, making the grade suitable for applications requiring excellent wear resistance, such as cutlery and ball bearings. It provides good corrosion resistance.
1. 440C Steel Chemical Composition
The standard chemical composition limits are detailed below:
Component | % |
Carbon (C) | 0.95 – 1.20 |
Chromium (Cr) | 16.0 – 18.0 |
Manganese (Mn) | 1.00 max |
Silicon (Si) | 1.00 max |
Molybdenum (Mo) | 0.75 max |
Phosphorus (P) | 0.040 max |
Sulfur (S) | 0.030 max |
2. 440C Steel Mechanical Properties:
- This steel achieves high hardness, typically 56-58 HRC annealed, reaching up to 58 HRC after heat treatment.
- Quenching from 1050°C in oil yields 60 HRC. A subsequent cold treatment at -75 °C for 1 hour can increase this to 61.5 HRC.
- Tempering reduces hardness: 150°C tempering results in 61 HRC; 200°C tempering yields 59 HRC.
- Per ASTM A 276-03, the maximum hardness for annealed (A condition) cold-finished 440B and 440C bar/shape is 285 HB.
- JIS G 4303:1998 specifies a minimum hardness of 56 HRC for hot-finished (HF) SUS440B (Q ≤ 75) and 58 HRC for SUS440C under the same conditions.
3. 440C Steel Physical Properties:
Key physical properties are listed here:
Property | Value |
Approximate Critical Temperatures | |
Ac1 (start of austenite formation on heating) | 815-865°C |
Ar1 (start of ferrite/carbide formation on cooling) | 765-665°C |
Ms (start of martensite formation) | 145°C |
Thermal Conductivity (at 20°C) | 29.3 W/(m·K) |
Coefficient of Linear Expansion (20 to 100°C) | 10.5 μm/m·K |
Coefficient of Linear Expansion (20 to 200°C) | 10.5 μm/m·K |
Coefficient of Linear Expansion (20 to 300°C) | 10.5 μm/m·K |
Coefficient of Linear Expansion (20 to 500°C) | 11.7 μm/m·K |
4. Applications
- Cutlery: High hardness allows for a durable sharp edge, while corrosion resistance withstands food and washing. Therefore, it is common for high-quality knife blades.
- Bearings: Its high hardness and wear resistance make it suitable for ball bearings and components, especially where corrosion resistance is also required. It is specified as a wear—and corrosion-resistant bearing steel.
- Surgical and Dental Instruments: The combination of high hardness (edge retention), wear resistance (longevity), and good corrosion resistance (withstanding sterilization/bodily fluids) makes 440C appropriate for surgical and dental tools.
- Valve Components: 440C’s corrosion resistance against various media and wear resistance against fluid flow support its use in nozzles and valve parts.
- Plastic Molds: High strength, hardness, and corrosion resistance make 440C a common choice for plastic molds.
- Marine Applications: High chromium levels provide sufficient corrosion resistance for use in marine atmospheres or seawater environments, though limitations exist.
- Applications Requiring High Wear Resistance: Generally, the high carbon content makes 440C a preferred stainless steel option where higher wear resistance is primary.
- Components for Corrosive Environments: AISI 440C is widely used where corrosion resistance is a key consideration.
5. Heat Treatment
Recommended heat treatment process for 440C steel:
5.1 Forging
Post-forging, higher-carbon grades like 440C require slow, careful cooling to prevent cracking. An interrupted cooling cycle might be employed: air cool to 150-250°C, reheat to ~650°C, then finally cool. This minimizes excessive grain-boundary carbide formation.
5.2 Austenitizing
Heat to a suitable temperature, typically 1038-1040°C (1900°F), to transform the microstructure to austenite and achieve optimal hardness/corrosion resistance. Hold at temperature to ensure adequate carbide dissolution.
5.3 Quenching
Rapid cooling after austenitizing forms martensite. Oil quenching or air quenching are standard methods, depending on section size and desired cooling rate.
5.4 Tempering
Quenched martensite requires tempering to reduce brittleness and increase toughness while maintaining sufficient For 440C, temper between 200°C and 350°C (approx. 400°F to 660°F). The specific temperature dictates the final hardness/toughness balance.
5.5 Tempering at 204°C (400°F)after austenitizing and oil quenching is a standard practice to optimize hardness and corrosion resistance.
- Tempering between 400°C and 600°C is generally avoided as it can cause sensitization (precipitation of coarser chromium carbides), reducing corrosion resistance.
- Stress Relieving: To reduce internal stresses, perform stress relief after forging or heavy machining. For hardened material, stress relief is slightly lower (14 to 28°C or 25 to 50°F) than the last tempering temperature.
6. 440C Steel’s Corrosion Resistance
6.1 Carbide Formation & Chromium Depletion:
Coarse eutectic carbide formation (during solidification and heat treatment) binds significant chromium, reducing the ‘free’ chromium available in the martensitic matrix for the protective passive layer. This affects overall corrosion resistance compared to lower-carbon stainless steels.
6.2 Comparison to Other Martensitic Grades:
Compared to grades like 420, 440C offers higher wear resistance (due to more carbides) but potentially slightly lower corrosion resistance in some environments due to chromium depletion. It is still considered to have good corrosion resistance.
6.3 Influence of Heat Treatment: Proper heat treatment is critical.
- Austenitizing aims to dissolve carbides and maximize chromium in solution, though based on the carbon content, undissolved carbides will remain.
- Lower temperature tempering (200°C-350°C) is recommended to balance hardness and corrosion resistance.
- Avoid tempering between 400°C-600°C, as this causes sensitization(coarser chromium carbide precipitation) and impairs corrosion resistance.
6.4 Performance in Specific Environments:
- Passivated 440C showed no rusting in tap water immersion tests.
- Conventional 440C can develop rust in 3.5% NaCl solution immersion tests, unlike some newer nitrogen-alloyed steels.
- Generally, achieving good corrosion resistance through hardening steel requires at least 10-11% ‘free’ chromium in the matrix post-heat treatment. High-carbon steels like 440C need excess chromium in the initial alloy to meet this.
6.5 Applications Context
Despite the carbon effect, 440C is widely used where high hardness, wear resistance, and reasonable corrosion resistance are needed (e.g., cutlery, bearings). However, compared to other stainless grades or specialized alloys, it may not be the optimal choice for severely corrosive environments (e.g., constant saltwater exposure).
FAQs
1. Is 440C a Japanese steel?
No, 440C is an American designation (AISI/ASTM).
2. Is D2 or 440C better?
- Choose D2 for maximum abrasive wear resistance where corrosion is minor or the environment is mild (e.g., cold-work tooling, long-run dies). D2 offers superior wear resistance and dimensional stability for such applications.
- Choose 440C for a balance of good wear resistance and significant corrosion resistance (e.g., molds, cutlery, and bearings in moist or mildly chemical environments).
3. Is 440C steel good for a knife?
Yes, its combination of hardness, wear resistance, and corrosion resistance makes 440C a very suitable and popular material for many knives.
Explore Our Other Products
D2/1.2379/SKD11
D3/1.2080/SKD1
D6/1.2436/SKD2
A2/1.23663/SKD12
O1/1.2510/SKS3
O2/1.2842
S1/1.2550
S7/1.2355
DC53
H13/1.2344/SKD61
H11/1.2343/SKD6
H21/1.2581/SKD7
L6/1.2714/SKT4
M2/1.3343/SKH51
M35/1.3243/SKH55
M42/1.3247/SKH59
P20/1.2311
P20+Ni/1.2738
420/1.2083/2Cr13
422 stainless steel
52100 bearing steel
440C stainless steel
4140/42CrMo4/SCM440
4340/34CrNiMo6/1.6582
4130
5140/42Cr4/SCR440
SCM415
Precision 440C Stainless Steel – Wear Resistance You Can Rely On
✅ Direct from Aobo Steel Manufacturer – Best factory prices, no middlemen
✅ Polished or Annealed Options – Delivered to your exact requirements
✅ Tight Tolerance Cutting – Save machining time and reduce waste
✅ Global Shipping – Secure delivery to your location
✅ Bulk Discounts Available – Competitive pricing for large-volume buyers
✅ Free Technical Support – Get expert advice on heat treatment, hardness, and corrosion resistance