D2 vs. A2 tool steel

D2 tool steel and A2 tool steel are often used in industrial production. This article compares the data of the two steels so that the user can choose in practice. So, let’s look at the following article about D2 vs. A2 tool steel!

D2 TOOL STEEL
D2 TOOL STEEL
A2 TOOL STEEL
A2 TOOL STEEL

D2 and A2 tool steel equivalent grades

USA/ASTMUSA/UNSGermany/DINGermany/W-Nr.Japan/JISISOChina/GB
D2T30402X155CrMo12-11.2379SKD11160CrMoV12Cr12Mo1V1
A2T30102X100CrMoV5-11.2363SKD12100CrMoV5Cr5Mo1V

Comparison of D2 and A2 composition

GradeC (%)Cr (%)Mo (%)V (%)Si (%)Mn (%)P (%)S (%)
D2 1.40 ~ 1.6011.00 ~ 13.000.70 ~ 1.200.50 ~ 1.100.10 ~ 0.600.10 ~ 0.60
A20.95 – 1.054.80 – 5.500.90 – 1.400.15 – 0.350.10 – 0.500.40 – 1.00≤0.030≤0.030

Manufacturing and service characteristics of D2 and A2

GradesResistance to DecarburizationHardening ResponseAmount of DistortionResistance to CrackingApproximate Hardness (HRC)MachinabilityToughnessResistance to SofteningResistance to Wear
D2MediumDeepLowestHighest54-61LowLowHighHigh to very high
A2MediumDeepLowestHighest57-62MediumMediumHighHigh

Relative Wear Resistance of D2 and A2

GradesHardness, HRCAbrasion weight loss, g x 10Relative weight lossWear resistance rating
D262.39.16:18
A262.93322:16

Wear resistance and toughness for cold-work dies and punches for blanking

GradesWear resistanceToughness
D282
A265

For cold extrusion

ApplicationsGradesWear resistanceToughnessWorking hardness, HRC
PunchesD28260-62
Punch shank or mandrelA26556-58
Die InsertD28260-62
Die BaseA26554-56
Die AnvilD28258-60
A26558-60