Your Trusted H13 Tool Steel Supplier

Leading Supplier of H13 Hot Work Tool Steel: Benefit from our extensive experience and commitment to excellence in H13 supply.

Aobo Steel supply H13 tool steel for your project

What is H13 tool steel? It is an air-hardening hot work tool steel and is one of the most widely used steels among all hot work tool steels. Compared to H11 tool steel, this steel offers higher thermal strength and hardness. Additionally, since it can be air-hardened, it exhibits low quenching deformation and residual stress and a minimal tendency for surface oxidation. Furthermore, it can produce secondary hardening, boasts excellent thermal stability, and effectively resists the erosion of aluminum alloy molten liquid.

Manufacturers widely use this steel to produce hot extrusion dies and mandrels, forging dies for drop hammers, and forging press dies. Additionally, it is commonly utilized for inserts in precision forging machines and die-casting molds for aluminum, copper, and their alloys. This versatility makes it a preferred choice for demanding industrial applications.

The designation in the U.S. ASTM A681 system is H13, and the name in the American AISI system is AISI H13 steel. Similarly, other national standards use comparable designations, such as ISO 40CrMoV5, Japan/JIS SKD61, USA/UNS T20813, Germany/DIN X40CrMoV5-1, Germany/W-Nr. 1.2344, and Czech Republic (CSN) 19554. For consistency, we will use H13 steel as a substitute in the following article. Next, we will discuss the properties of H13 tool steel in detail.

h13 TOOL STEEL

H13 tool steel Applications

Extrusion Dies
Die Casting Dies
m35 steel cold forging dies
Shear Blades

1. Die Casting Dies:
H13 die steel exhibits excellent heat resistance and toughness, making it ideal for die-casting dies. Specifically, workers inject molten metal under high pressure and temperature during the die-casting process, requiring materials capable of withstanding extreme conditions.

2. Forging Dies:
H13 handles high impact and mechanical stress effectively, making it suitable for forging dies that shape metals at high temperatures. Additionally, its durability and resistance to thermal fatigue ensure reliable performance in demanding industrial applications.

3. Extrusion Dies:
H13 is strong and resists wear. This makes it useful for extrusion dies. These dies shape materials are under high pressure.

4. Plastic Molding Dies:
Manufacturers commonly use H13 tool steel to make molds for plastic injection because they need its heat resistance and wear resistance.

5. Hot Shear Blades:
Its ability to stay sharp at high temperatures makes it a great material for hot shear blades used in metal cutting processes.

6. Aluminum alloy building material mold materials:
Chinese industries widely use H13 as a mold material for aluminum alloy building materials, which is why people call it H13 mold steel.

H13 Steel: High-Temperature Excellence


H13 steel delivers superior strength, thermal fatigue resistance, and hardness above 500°C—ideal for die-casting molds, hot-working dies, and high-temperature fixtures. Trusted in aluminum and magnesium alloy die-casting, forging, and extrusion, it’s your go-to choice for peak performance.

H13 tool steel overview

H13 steel is a widely used hot work tool steel globally. It is renowned for its strength and toughness, high hardenability, and resistance to thermal cracking. This steel features higher levels of carbon and vanadium, which result in good wear resistance but relatively lower toughness. It offers good heat resistance, maintaining strong strength and hardness, high wear resistance, and toughness at elevated temperatures. Furthermore, it has excellent overall mechanical properties and high tempering resistance.

Chemical composition

Carbon (C)Chromium (Cr)Molybdenum (Mo)Vanadium (V)Silicon (Si)Iron (Fe)Nickel (Ni)Copper (Cu)Manganese (Mn)
0.32 – 0.454.75 – 5.501.10 – 1.750.80 – 1.200.80 – 1.20≥ 90.9≤ 0.3≤ 0.25Smaller amounts

Physical properties

PropertyValue
Density7.75 – 7.80 g/cm3
Tensile Strength, Ultimate1200 – 2050 MPa (174000 – 231000 psi)
Tensile Strength, Yield1000 – 1380 MPa (145000 – 200000 psi)
Hardness45-52 HRC (Rockwell C Hardness)
Impact Toughness20-40 J/cm2
Compressive Strength2550 MPa

1. Pre-heating

a) Forging Process Specifications

ItemHeating Temperature (°C)Forging Temperature (°C)Finishing Temperature (°C)Cooling Method
Ingot1140-11801100-1150900-850Slow cooling (sand or pit cooling)
Billet1120-11501050-1100900-850Slow cooling (sand or pit cooling)
 

b) Heat Treatment Process

Pre-Heat Treatment PlanProcess Parameters
Annealing ProcessHeating temperature: 860 ~ 890°C, hold for 3 ~ 4 hours, furnace cool to below 500°C and then air cool, hardness after annealing ≤229HBW, structure: spheroidized pearlite + a small amount of carbides
Stress Relief AnnealingHeating temperature: 730 ~ 760°C, hold for 3 ~ 4 hours, furnace cool

c) Hardness and Microstructure Before and After Annealing

ConditionIndentation Diameter (mm)HBWMicrostructure
Before Annealing≈2.75≈500Martensite or Bainite
After Annealing≥3.9≥241Spheroidized Pearlite + Small Amount of Carbides
 

2. Quenching

a)Recommended Tempering Process Specification

Quenching Temperature (°C)CoolingQuenching MediumQuenching Medium Temperature (°C)Cooling toHardness (HRC)
1020 ~ 1080 Oil or Air20 ~ 60Room Temperature56 ~ 58
 

b)Relationship between quenching temperature, hardness, and grain size

Quenching Temperature (°C)930950980100010201040106010801100
Hardness (HRC)50.35253.554.856.357.858.259.159.1
Grain Size (Level)11.211.111.111.1111087
 

3. Tempering

a)Recommended Tempering Process Specifications

PurposeTempering Temperature (°C)EquipmentCooling MethodTempering Hardness (HRC)
Relieve stress, reduce hardness560 ~ 580Melting salt bath furnace or air furnaceAir cooling47 ~ 49
 

b)The relationship between tempering temperature and hardness

Tempering Temperature (°C)Hardness (HRC)
10059.0
20057.0
30054.5
40054.5
45057.5
50057.5
55053.5
60049.5
65040.0
70030.0

From forging to extrusion, H13 steel delivers unmatched strength and versatility. Discover the difference today!

H13 steel equivalents: DIN 1.2344 and JIS SKD61

Under the German and Japanese standard systems, DIN 1.2344 and SKD61 are steels that can substitute H13. They share similar compositions and properties, and are internationally recognized air-hardening hot work die steels. These steels exhibit excellent high-temperature strength, toughness, and resistance to thermal fatigue, enabling them to withstand rapid temperature changes. They are suitable for prolonged operation under high-temperature conditions while maintaining superior machinability and polishing performance.

Introduction to DIN 1.2344 steel

Chemical composition

Carbon (C)Silicon (Si)Manganese (Mn)Chromium (Cr)Molybdenum (Mo)Vanadium (V)Phosphorus (P)Sulfur (S)
0.35 – 0.420.8 – 1.20.25 – 0.54.8 – 5.51.2 – 1.50.85 – 1.15≤0.030≤0.030

1.2344 material properties

  • Machinability: Machine 1.2344 tool steel, which has moderate machinability, best in its annealed condition. Use proper cutting fluids and tools to reduce tool wear.

  • Weldability: Welding 1.2344 steel presents some challenges. To prevent cracking, welders must carefully preheat the material and perform post-weld heat treatment. Maintaining weld integrity requires specialized welding techniques.

Introduction to JIS SKD61 steel

Chemical composition

Carbon (C)Chromium (Cr)Molybdenum (Mo)Vanadium (V)Manganese (Mn)Silicon (Si)Phosphorus (P)Sulfur (S)
0.32 – 0.424.50 – 5.501.00 – 1.500.80 – 1.200.20 – 0.500.80 – 1.20≤ 0.03≤ 0.03

Physical Properties

PropertyValue
Density7.8 g/cm³
Thermal Conductivity28 W/m·K at 100°C
Elastic Modulus210 GPa
Specific Heat Capacity460 J/kg·K
Hardness (After Heat Treatment)50 – 55 HRC
thไทย