H11 vs H13 Steel: A Detailed Comparison of Two Essential Hot-Work Die Steels

Estimated reading time: 10 minutes

Key Takeaways

  • H11 and H13 steels are both AISI hot-work tool steels known for their high strength and hardness at elevated temperatures.
  • H13 has a higher vanadium content, enhancing its wear resistance compared to H11, which offers better toughness.
  • Both steels require specific heat treatment processes, including preheating and air cooling, to achieve optimal performance.
  • Applications vary: H13 excels in high-wear environments, while H11 is preferred where toughness is critical.
  • The choice between H11 vs H13 steel depends on the specific needs for wear resistance and toughness in applications.

H11 and H13 steels both belong to the American Iron and Steel Institute (AISI) H series of hot-work tool steels, representing two of the most widely used 5% chromium hot-work tool steels. These steels are critical materials in manufacturing, with their core advantage being the ability to maintain excellent strength and hardness even under high-temperature working conditions.

Although they share fundamental similarities in properties, subtle differences in chemical composition grant each distinct performance advantages. Therefore, in practical applications, the choice between H11 and H13 should be made carefully based on the specific operating conditions of the mold and the required service life.

H11 and H13 are both medium-alloy air-hardening steels or ultra-high-strength steels. Through appropriate heat treatment processes, their 0.2% proof strength can be elevated to levels far exceeding 1380 MPa.

Classification and Shared Metallurgical Foundation

H11 and H13 both belong to the H10-H19 chromium-based hot-work steel subcategory. They share the same metallurgical foundation, characterized by a medium carbon content and high concentrations of chromium and other carbide-forming elements.

H11 vs. H13 Equivalent Grades:

US(AISI)Germany (DIN / W-Nr.)Japan (JIS)China (GB)UK (BS)
H111.2343(X37CrMoV5-1)SKD64Cr5MoSiVBH11
H131.2344(X40CrMoV5-1)SKD614Cr5MoSiV1BH13

These two types of steel share three key characteristics:

First, they are used in high-temperature hot-working applications, such as aluminum alloy die casting, and can withstand operating conditions up to 600°C.

Second, they all exhibit extremely high hardenability and are air-hardening steels. Even large steel components can be fully hardened from the inside out simply by cooling in air. Air cooling minimizes internal stresses and dimensional changes generated during heat treatment.

Finally, both H11 and H13 are secondary hardening steels. They must be tempered at temperatures above approximately 510°C to precipitate fine alloy carbides, thereby achieving optimal performance. This high-temperature tempering process not only effectively relieves stress but is also the key reason they maintain stable performance during high-temperature operation. The upper limit of this high-temperature operation must remain below the tempering temperature.

Chemical Composition: The Vanadium Difference

The core difference between H11 and H13 steels lies primarily in their Vanadium (V) content.

H11 and H13 composition

AISIUNS No.DINC (%)Mn (%)Si (%)Cr (%)Ni (%)Mo (%)V (%)
H11T208111.23430.33-0.430.20-0.500.80-1.204.75-5.500.30 max1.10-1.600.30-0.60
H13T208131.23440.32-0.450.20-0.500.80-1.204.75-5.500.30 max1.10-1.750.80-1.20

This difference in Vanadium content is the major differentiator in mechanical performance:

FeatureH11H13
Vanadium (V) ContentLower (e.g., 0.30–0.60%)Higher (e.g., 0.80–1.25%)
Wear ResistanceGoodHigher, due to V carbides
ToughnessHigher/Better Fracture ToughnessSlightly Lower
Hot Hardness/Temper ResistanceExcellentSlightly Better

Performance Showdown: Mechanical Properties

The primary difference in mechanical properties between H11 and H13 stems from their chemical compositions, with H13 possessing a higher vanadium content.

In terms of wear resistance, H13 offers superior performance. Its higher vanadium content promotes the formation of abundant hard vanadium carbides, resulting in wear resistance that surpasses H11. This makes it highly suitable for high-wear applications such as hot forging or hot extrusion.

However, H11 offers superior toughness. The carbide particles used in H13 to enhance wear resistance sometimes come at the expense of some toughness. Therefore, H11 exhibits higher fracture toughness.

In terms of heat hardness, both perform excellently, but H13 holds a slight edge. This is again due to H13 containing more vanadium.

Heat Treatment and Quality Manufacturing

The heat treatment processes for H11 and H13 are critical for maximizing their performance. As both are air-hardening steels, their fundamental heat treatment steps are highly similar, typically including preheating, austenitizing, quenching, and subsequent secondary or tertiary high-temperature tempering.

Standard Heat Treatment

First comes preheating, where the steel should be preheated to between 790°C and 815°C before being uniformly heated to the final forging or austenitizing temperature.

The austenitizing temperature range for H11 steel typically falls between 995°C and 1025°C, while the austenitizing temperature for H13 steel is slightly higher, generally between 995°C and 1040°C. During this step, a controlled protective atmosphere must be employed to prevent decarburization of the steel surface.

Quenching is the third step. H11 and H13 must be cooled in air, as this method ensures minimal residual stress within the material. These steels must never be water-quenched.

Finally, tempering. To achieve secondary hardening and relieve stress, secondary tempering or multiple tempering cycles are strongly recommended. The tempering temperature must exceed the secondary hardening peak of 510°C. For H13 steel specifically, tempering within the 565°C to 650°C range optimizes its secondary hardening effect.

Quality Enhancement (ESR/VAR)

To meet the demands of demanding applications, H11 and H13 steel grades are often subjected to specialized manufacturing processes to enhance their quality and performance further.

In terms of enhancing melting quality, these two steels often employ melting technologies such as electroslag remelting (ESR) or vacuum arc remelting (VAR). 

Compared to conventionally melted steels, the ESR or VAR process significantly enhances material ductility and toughness. The VAR process, in particular, achieves extremely low impurity levels and high microstructural uniformity. For high-performance H13 die-casting molds or injection molds, ESR remelting has become a common manufacturing requirement. Our company offers ESR H13 and H11 materials.

Surface Modification

For surface performance enhancement, both H11 and H13 steels typically undergo nitriding treatment. Nitriding is a chemical heat treatment that forms an extremely hardened layer on the steel surface.H11 and H13 achieve high core strength and high surface hardness after nitriding. H13, in particular, exhibits excellent responsiveness to nitriding, with surface hardness reaching 1000-1200 HV. Furthermore, H13’s outstanding resistance to high-temperature tempering ensures that its internal core maintains its original high strength without softening during nitriding heating.

Applications and Selection Criteria

When choosing between H11 and H13, the decision essentially involves balancing H13’s high wear resistance against H11’s high toughness.

  • Die Casting Applications: Both are industry benchmarks. H13 has the broadest application range, commonly used for die casting of aluminum, zinc, and magnesium alloys, while H11 is frequently used for die casting of aluminum and lead.
  • Hot Forging and Extrusion: H13 is the more versatile choice for hot-work forging dies. H11 is commonly used for punches and dies in aluminum forging (HRC 44-48) or for small-batch hot-rolled rolls.
  • Plastic molds: Both materials are suitable. H13 is the superior choice, particularly ESR remelted H13, which is the preferred option for manufacturing high-polish precision molds such as automotive lenses. H11 is suitable for high-temperature plastic molding applications where operating temperatures exceed 300°C.
  • Aerospace Structural Components: Both are ultra-high-strength alloys. H11 is more commonly used in high-stress components such as aircraft landing gear and rocket casings, as it must maintain high strength at elevated temperatures. H13 was also widely used in the past, but its application in this field has declined with the advent of new high-toughness steels.

Summary for Selection:

Choose H13 when:

  • When high wear resistance is the primary requirement, H13 contains higher levels of vanadium (V), enabling the formation of more dispersed, hard vanadium carbides. This makes it superior to H11 in abrasive wear environments such as hot extrusion and high-wear forging.
  • When optimal red hardness and resistance to tempering are required, H13 offers slightly superior stability at elevated temperatures, better preserving hardness and strength under high-heat conditions.
  • For general-purpose hot work and die casting molds, H13 remains the most widely used general-purpose hot work tool steel, particularly in die casting mold applications.

Choose H11 when:

  • When maximum toughness is required, H11 offers superior fracture toughness and ductility compared to H13, making it a safer choice for applications involving impact loads where preventing unexpected mold cracking is critical.
  • When used for high-strength structural components, H11 resists softening and maintains high strength at temperatures up to 540°C, making it commonly used in high-stress aerospace components such as landing gear.

Supplementary data

We have compiled authoritative data on H11 and H13, which we hope will be helpful to our readers.

Comparison of other parameters

FactorH11 tool steelsH13 tool steels
Usual Working Hardness, HRC38-5540-53(H13 steel hardness)
Depth of HardeningDD
Finest Grain Size at Full Hardness, Shepherd Standard88
Surface Hardness as-Quenched, HRC53-5551-54
Core Hardness (25 mm, or 1 in., diam round), HRC53-5551-54
Quenching MediumAA
Hardening Temperature, °C (°F)995-1025 (1825-1875)995-1040 (1825-1900)
Dimensional Change on HardeningLL
Safety on HardeningHH
Susceptibility to DecarburizationHH
Approximate Hardness as-Rolled or Forged, HB500500
Annealed Hardness, HB192-229192-229
Annealing Temperature, °C (°F)845-900 (1550-1650)845-900 (1550-1650)
Tempering Range, °C (°F)540-650 (1000-1200)540-650 (1000-1200)
Forging Temperature, °C (°F)1065-1150 (1950-2100)1065-1150 (1950-2100)

H11 and H13 tool steels share many similarities in terms of their mechanical properties, heat treatment characteristics, and forging capabilities. The primary difference lies in their hardness range, with H13 offering slightly higher hardness for more demanding applications. The choice between these two steels depends on the specific requirements of the intended application, such as the level of wear resistance, toughness, and dimensional stability needed.

Tensile Properties of H11 and H13 Tool Steels at Elevated Temperatures

Steel TypeTesting Temperature (°C)Testing Temperature (°F)Tensile Strength (MPa)Tensile Strength (ksi)Yield Strength (0.2% offset) (MPa)Yield Strength (0.2% offset) (ksi)Elongation (50 mm) (%)Reduction of Area (%)Room-Temperature Hardness (HRC) Before
testing 
Room-Temperature Hardness (HRC) After
testing 
H11RoomRoom180626214822151035.85050
1503001689245135819710.136.15050
260500160023213451959.834.55050
345650157922913171911035.25050
4258001510219128918711.438.75050
4809001427207114516612.238.95050
540100012411809651401135.45050
595110097914272410512.846.25047
6501200586854346318.966.65041
H13480900153122293752
54010001413205114352
59511001193173154952
6501200814118225952

Note:

  • The “-” in the Yield Strength columns for H13 steel indicates that the data was unavailable.
  • The Room-Temperature Hardness (HRC) column shows values before and after testing, separated by a comma.
  • Data from Teledyne VASCO. Allegheny Ludlum Industries, and Universal-Cyclops Steel Corp. 

CVN impact toughness of H11 and H13 tool steels as a function of testing temperature.

the relationship between testing temperature in Fahrenheit and Celsius, and impact strength in both Joules (J) and foot-pounds force (ft lbf) for two materials, H11 and H13

This graph suggests that H11 and H13 become more resistant to impact at higher temperatures. However, H13 is more sensitive to temperature changes, showing a more significant increase in impact strength with rising temperatures.