O2 tool steel has high hardness and wear resistance. It experiences minimal distortion during quenching and has excellent hardenability. This steel is suitable for making various precision measuring tools and templates. It is also used for smaller-dimension dies, cold press molds, engraving molds, and blanking dies. Additionally, it can be used for machine tool screws and other structural components.
The designation is O2 in the U.S. ASTM A681 system. Similar designations under other national standards include ISO 90MnV2, USA/UNS T31502, Germany/DIN 90MnCrV8, and Germany/W-Nr. 1.2842.
1. Applications
To provide a clearer picture, here’s a breakdown of typical industrial uses for O2 tool steel, highlighting where its properties deliver maximum benefit:
| Application Category | Specific O2 Steel Uses | Key Advantages for Your Operations |
|---|---|---|
| Dies and Punches | Blanking dies, trimming tools, drawing dies, flanging tools, forming punches. Notably effective for blank holders in stamping tools (resisting pressure and friction) and as ejectors and blank holders in deep drawing dies (withstanding friction). | Excellent wear resistance, good toughness, maintains dimensional stability for consistent part production. |
| Gages | Precision measurement tools, master gages. | High dimensional stability after hardening, crucial for accuracy; good wear resistance for longevity. |
| Machinery Components | Items like cams, durable bushings, and wear-resistant guides. | Offers the necessary wear resistance and toughness for demanding mechanical parts. |
| Coining & Powder Pressing | Tooling for coining operations, punches, and dies for powder metal compacting. | Withstands high compressive forces and abrasive wear common in these processes. |
| Cold Rolling | Rolls used in cold rolling applications. | Delivers the high wear resistance and toughness required for shaping metals at ambient temperatures. |
2. Chemical Composition of O2 Tool Steel
| Element | Symbol | Typical Content (%) | Notes |
| Carbon | C | 0.85 – 0.95 | Nominal: ~0.90%. Essential for hardness and wear resistance. |
| Manganese | Mn | 1.40 – 1.80 | Nominal: ~1.60%. The primary alloying element in O2; aids hardenability. |
| Silicon | Si | Max 0.50 | Nominal: ~0.25%. Acts as a deoxidizer. |
| Chromium | Cr | Max 0.50 | Nominal: ~0.22% or ~0.50%. Contributes to hardenability and wear resistance. |
| Vanadium | V | Max 0.30 | Nominal: ~0.20% or ~0.30%. Promotes fine grain structure and toughness. |
| Tungsten | W | Max 0.30 | Nominal: ~0.30%. Can improve wear resistance at higher temperatures. |
| Molybdenum | Mo | Max 0.30 | Nominal: ~0.30%. Increases hardenability and toughness. |
| Nickel | Ni | Max 0.30 | May be present in small amounts. |
| Phosphorus | P | Max 0.03 | Kept to a minimum as it can reduce toughness. |
| Sulfur | S | Max 0.03 | Kept to a minimum; can affect toughness but aids machinability in some steels. |
| Copper | Cu | Max 0.25 | Typically an impurity. |
| Iron | Fe | Balance | The remainder of the material. |
Note: Nominal values are approximate and can vary slightly between different sources or specific heats, but the overall composition remains within the defined ranges for AISI O2 grade.
The Impact of Composition on Performance
This specific combination of high carbon content and moderate alloying—particularly the notably higher manganese level compared to other O-series tool steels like O1—is what defines O2 tool steel. This formulation provides O2 with its excellent hardening characteristics when quenched in oil, leading to a good balance of wear resistance and toughness suitable for a variety of cold-work tooling applications.

Are you looking for O2 tool steel? Please fill out the following form to contact us for the most competitive O2 tool steel today!
3. O2 Tool Steel Properties
Here’s a breakdown of the key O2 steel properties and what they mean for your operations:
| Property Category | Description & Significance for Users |
|---|---|
| High Hardness | Achieves a notable surface hardness (60-62 HRC), critical for resisting indentation and maintaining a sharp cutting edge or durable forming surface in tooling. |
| Good Wear Resistance | The high carbon content and resultant hardness contribute to good resistance against abrasive wear, extending the service life of tools and dies. |
| Fair Toughness | Offers a balanced level of toughness suitable for many cold-work applications, helping to prevent premature chipping or fracture under operational stresses. |
| Good Non-Deforming Properties | Exhibits commendable dimensional stability with relatively low distortion after the oil-quenching heat treatment process. This is vital for precision tooling. |
| Good Safety in Hardening | The oil-quenching method used for O2 steel minimizes the risk of cracking and distortion compared to water quenching, especially beneficial for complex tool geometries. |
| Machinability | In its annealed (pre-hardened) state, O2 tool steel (similar to O1 in this regard) offers good machinability, facilitating easier tool fabrication. |
| Thermal Sensitivity | It’s important to note that O2 steel has poor resistance to softening at elevated temperatures. This characteristic firmly places it within the cold-work steel category, meaning it’s not intended for applications involving high heat. |
It cannot be overstated that the final mechanical properties of O2 steel are profoundly shaped by the specific heat treatment cycle employed. Factors such as the austenitizing temperature, quench rate, and subsequent tempering process are meticulously controlled to develop the desired hardness, toughness, and wear resistance.
4. O2 Tool Steel Heat Treatment
Achieving O2 tool steel’s hardness and wear resistance relies on a precise heat treatment process. As an oil-hardening cold-work steel, its exceptional properties are developed through controlled thermal cycling. For more information about this topic, please refer to the O2 tool steel heat treatment.
4.1 The Annealing Process
O2 tool steel is typically supplied annealed. This initial heat treatment softens the steel, relieves stresses, and refines its microstructure, making it easier to machine or prepare for cold forming.
For severe cold-forming, spheroidize annealing is preferred:
- Heat the steel near or slightly below its lower critical temperature (Ac1).
- Hold at this temperature for a prolonged period.
- Cool slowly. This process transforms carbides into a globular shape, resulting in maximum softness and ductility.
4.2 The Hardening Cycle
Hardening is the critical phase where O2 steel develops its characteristic high hardness. It involves heating to form austenite, then rapid cooling (quenching) to create a predominantly martensitic structure.
4.2.1 Preheating
While O2 is an oil-hardening grade, preheating is highly recommended, especially for larger sections or intricate parts, to minimize thermal shock and reduce distortion or cracking.
- Recommended Preheat Temperature: Around 650°C (1200°F).
- Tip: Placing the part on top of the furnace before preheating can help gradually raise its temperature.
4.2.2 Austenitizing
Austenitizing involves heating the steel to a specific temperature to fully transform its structure into austenite, allowing carbides to dissolve.
- Recommended Austenitizing Temperature for O2 Steel: 790–815°C (1454–1472°F). Some sources suggest 800°C (1475°F).
- Soaking Time: Hold for 30–45 minutes per 25mm (1 inch) of thickness to ensure uniform heating and carbide dissolution.
- Caution: Proper furnace atmosphere control to prevent excessive decarburization or oxidation.
4.2.3 Quenching in Oil
After austenitizing, O2 steel is rapidly quenched in oil to transform austenite into hard martensite.
- Quenching Medium: Oil is specific to O2 steel, offering effective hardening with less distortion risk than water, especially for complex shapes.
- Target Quench Temperature: Quench until the steel reaches approximately 66–93°C (150–200°F).
4.2 Tempering
As-quenched martensite is very hard but brittle and stressed. Tempering is an indispensable post-quench treatment to improve toughness and ductility, reduce hardness to the desired level, relieve internal stresses, and enhance dimensional stability.
Critical Timing for Tempering:
Temper O2 steel parts as soon as they reach 52–65°C (125–150°F) after quenching. Delaying can lead to cracking.
- Tempering Temperature: Commonly around 175°C (350°F) for O2 steel (similar to O1). The typical range is 149–232°C (300–450°F), depending on desired final hardness. Lower temperatures yield higher hardness; higher temperatures increase toughness but reduce hardness.
- Soaking Time: Soak for at least 2 hours per 25mm (1 inch) of the thickest section.
Multiple Tempering Cycles:
Multiple tempering cycles (typically two) are often recommended for O2 tool steel. A second temper (after cooling to room temperature from the first) further refines the microstructure, relieves more stress, and can transform retained austenite. Air cool to room temperature between cycles.
4.3 Optional Advanced Treatments for O2 Steel
For specific needs, consider these treatments:
4.3.1 Stress Relieving for Enhanced Stability
Stress relieving minimizes residual stresses from manufacturing (machining, forming). Heat below Ac1, hold, then cool slowly.
- Timing: Before hardening, or after hardening and tempering.
- If Post-Hardening: Use a temperature ~25°C (50°F) below the final tempering temperature to avoid over-softening.
4.3.2 Sub-Zero Treatment (Cryogenic Treatment)
Sub-zero treatment can transform retained austenite (untransformed during quenching) into martensite by cooling to very low temperatures (e.g., -75°C / -103°F or lower). This may increase hardness and dimensional stability.
- Critical Post-Treatment: If used, O2 steel must be tempered immediately after use to relieve stresses from the new martensite and improve toughness.
4.4 Summary of O2 Steel Heat Treatment Parameters
A quick reference for the typical O2 steel heat treatment process:
| Process Step | Temperature Range | Typical Duration/Key Notes | Primary Purpose |
| Annealing | (Spheroidize) Near/slightly below Ac1 | Prolonged heating, slow cooling | Maximize softness, improve machinability |
| Preheating | ~650°C (1200°F) | Until uniform temperature | Minimize thermal shock, reduce distortion risk |
| Austenitizing | 790–815°C (1454–1472°F) | 30–45 min per 25mm (1 inch) of section | Form austenite, dissolve carbides |
| Quenching (Oil) | Cool to 66–93°C (150–200°F) | Rapid cooling in oil | Transform austenite to martensite |
| Tempering | 149–232°C (300–450°F) (e.g., 175°C / 350°F typical) | Min. 2 hrs per 25mm (1 inch) section. Temper ASAP once part reaches 52-65°C (125-150°F). | Improve toughness, reduce brittleness, relieve stress. Multiple tempers often best. |
| Stress Relieving | (If post-hardened) ~25°C (50°F) below tempering temp. | Hold, then slow cool | Relieve manufacturing stresses |
| Sub-Zero Trt. | Very low (e.g., -75°C / -103°F) | – | Transform retained austenite. Temper immediately after. |
Adhering to these O2 steel heat treatment recommendations is essential for achieving target hardness (typically 60–62 HRC) and optimal performance.
FAQs
O2 steel is an oil-hardening cold-work tool steel with high carbon and a moderate alloy content, known for its high hardness, good hardenability, and relatively low dimensional changes during heat treatment.
O2 steel has better hardenability and less heat-treat distortion than O1 steel due to its higher manganese content, giving it an advantage in some precision mold applications. O1 steel may be more attractive in terms of versatility and cost.
O2 steel is good for knives, especially those with high heat treatment distortion requirements.
Germany DIN: The German DIN standard material number 1.2842
Looking for Premium O2 Tool Steel?
At Aobo Steel, we leverage over 20 years of specialized forging experience to deliver top-tier O2 tool steel, precisely tailored to your application needs. Our expert team is dedicated to helping you find the optimal material solution.
Ready to enhance your project? Please fill out the form below to connect with us for a personalized quote or expert consultation.