AOBO STEEL: Your Trusted Supplier of D3 Tool Steel

Reliable D3 Tool Steel for Manufacturers

Our company, Aobo Steel, is a professional D3 tool supplier and stockist. We maintain a standing inventory of D3 round bars.

What is D3 tool steel? D3 steel exhibits high strength, good hardenability, and excellent wear resistance. It undergoes minimal distortion during quenching. However, it has poor impact toughness and is prone to brittle fracture. It quickly forms uneven eutectic carbides and has poor thermal conductivity and high-temperature plasticity.

D3 steel’s excellent wear resistance makes it a popular choice for manufacturing cold stamping dies and punches, cold cutting tools, drill bushings, gauges, drawing dies, embossing dies, thread rolling plates, deep drawing dies, and thread rolling dies. These applications demand high wear resistance and typically involve lower impact loads.

D3 tool steel is a widely used high-carbon, high-chromium cold work tool steel. D3 is the designation under the ASTM A681 standard. Similar grades in other common standards include Germany/W-Nr. 1.2080, USA/ASTM T30403, Japan/JIS SKD1, and Czech Republic/CSN 19436. 

d3 tool steel
1.2080 tool steel

D3 tool steel Applications

die holders
kitchen knives
Shear Blades
Thread rolling dies

D3 tool steel is excellent for jobs requiring strong wear resistance and hardness. It works well in harsh, abrasive conditions. Some of its typical applications include:

  • Blanking and Punching Dies: D3 steel makes tools subject to high stress and wear, including blanking dies, punching dies, and forming dies.
  • Shear Blades: High hardness and toughness make it suitable for shearing softer metals.
  • Rolls and Slitting Tools: Manufacturers frequently choose D3 steel for rolling and slitting operations where high wear resistance is crucial.
  • Cold Work Tooling: Manufacturers use D3 tool steel for tools in heavy cold working processes, such as hobbing dies and forging dies.

Fast Delivery, Factory Direct

We pride ourselves on delivering your materials quickly and directly from our factory to your door. No middlemen, no delays—just fast and reliable service. We understand that time is of the essence when it comes to completing your projects, so we make sure to expedite our delivery process and get your materials to you as soon as possible.

Introduction to D3 tool Steel

D3 steel chemical composition ​

ElementCarbon (C)Chromium (Cr)Molybdenum (Mo)Vanadium (V)Manganese (Mn)Silicon (Si)Phosphorus (P)Sulfur (S)
Percentage (%)2.00 – 2.3511.00 – 13.50≤ 0.40≤ 0.35≤ 0.60≤ 0.60≤ 0.03≤ 0.03

D3 tool stee heat treatment​

1. Preheating Treatment Process Specifications

 Process Parameters
General Annealing After ForgingHeating temperature: 850 ~ 870°C, holding time: 4 ~ 5h, cooling rate: <30°C/h, furnace cooling to below 500°C, air cooling after furnace, hardness after annealing: ≤229HBW, microstructure after annealing: granular pearlite + carbides
Isothermal Annealing After ForgingHeating temperature: 830 ~ 850°C, holding time: 2 ~ 3h, furnace cooling to 720 ~ 740°C, holding time: 3 ~ 4h, furnace cooling to below 550°C, air cooling after furnace, hardness after annealing: ≤269HBW, microstructure after annealing: granular pearlite + carbides

2. Quenching

a)Recommended Quenching Specifications

ProcessQuenching Temperature (°C)Cooling MethodHardness HRC
Recommended Quenching Specifications950 ~ 980Oil Cooling≥60

b)Performance Comparison under Different Heat Treatment Processes

Heat Treatment ProcessHardness (HRC)Impact Toughness a_k’ (J/cm²)Retained Austenite (Volume Fraction, %)Die Life (×10⁵ pieces)Wear Amount (mg)
980°C Heating, Oil Quenching66.514.113.24
980°C Heating, 180°C Tempering 50 min65.815.85
980°C Heating, 270°C Tempering 3h65.515.9611.9
980°C Heating, 270°C Tempering 4h6017.715.02
980°C Heating, 270°C Tempering 5h5916.8
980°C Heating, 180°C Pre-tempering 35 min, 270°C Tempering 3h64.614.612-158.2
980°C Heating, 180°C Pre-tempering 35 min, 270°C Tempering 4h46.214.912-28
980°C Heating, 180°C Pre-tempering 35 min, 270°C Tempering 3h (Repeated)63.815.2

c)Relationship between Quenching Temperature and Hardness

Quenching Temperature (°C)Hardness (HRC)
87554.5
90057
92560
95062.5
97565
100066
105064
110059.5

 3. Tempering

a)Recommended Tempering Process Specifications

Purpose of TemperingHeating Temperature (°C)Tempering Time (hours)Number of Tempering CyclesHardness (HRC)
Relieve stress, stabilize structure180 ~ 2002160 ~ 62
Relieve stress, reduce hardness320 ~ 3502157 ~ 58

b)Relationship between Tempering Temperature and Hardness

Tempering Temperature (°C)Not Tempered200300400450500550600650
Hardness (HRC)65636260606059.557.144

D3 vs D5 steel

D3 and D5 steels are both high-carbon, high-chromium cold work tool steels with high hardness and wear resistance after hardening and tempering. Their differences include hardening methods, wear resistance and toughness, heat treatment distortion, and applications.

  • Hardening method: D3 steels are usually oil quenched, D5 steels are air-cooled and hardened.
  • Wear resistance and toughness: D3 steel has better wear resistance, while D5 steel has better toughness.
  • Heat treatment distortion: D5 steels are characterized by the smallest heat treatment distortion of the D series steels. Since D5 steels can be air-cooled and hardened, this usually results in less distortion than that caused by oil or water cooling.D3 steels, although also classified as low distortion steels, are more susceptible to distortion during hardening, as they usually require oil quenching.
  • Applications: Both steels are suitable for various cold work applications such as blanking dies and forming dies. The high wear resistance of D3 steel and the low heat distortion of D5 steel make D3 steel suitable for applications where very high wear resistance is more desirable, and D5 steel is more suitable for precision mold making.

Comprehensive Support

Enjoy 24-hour service responses, customizable solutions such as cutting to specification, and support for independent third-party testing. We’re here to ensure your experience is seamless. Our team of experts is always available to assist with any questions or concerns.

What are the D3 tool steel equivalents? DIN 1.2080 and JIS SKD1

1.2080 and SKD1 are steels similar to D3 from the German and Japanese standard systems, respectively, and they can be used interchangeably. They are high-carbon, high-chromium ledeburite steels with high strength. They possess good hardenability, small quenching deformation, and good wear resistance. The hardness after quenching is at least 60 HRC. Due to the carbon content in the steel being up to 2.30%, the steel becomes hard and brittle, resulting in poor impact toughness. It can barely withstand large impact loads and is prone to brittle fracture, and moreover, it tends to form inhomogeneous eutectic carbides.

They are the most common type of tool steel in China and are also a type of mold steel that our company keeps in regular stock. Because the content of expensive alloys is not high, their price is basically the lowest among tool steels.

Introduction to DIN 1.2080 steel

1.2080 Chemical Composition

Carbon (C)Chromium (Cr)Manganese (Mn)Silicon (Si)Phosphorus (P)Sulfur (S)
2.00 – 2.20%11.00 – 13.00%0.20 – 0.40%0.10 – 0.60%≤ 0.030% (max)≤ 0.030% (max)

1.2080 Mechanical Properties:

Hardness: 58-64 HRC (Rockwell Hardness)
Impact Toughness: 28 J/cm²
Modulus of Elasticity: 190-210 GPa
Poisson’s Ratio: 0.27-0.30

Introduction to JIS SKD1 steel

SKD1 Chemical Composition

Carbon (C)Chromium (Cr)Manganese (Mn)Silicon (Si)Vanadium (V)Phosphorus (P)Sulfur (S)
1.40 – 1.6011.00 – 13.000.20 – 0.400.10 – 0.400.15 max≤ 0.030≤ 0.030

SKD1 Physical Properties

PropertyValue
Density7.75 g/cm³
Thermal Conductivity20.0 W/m·K
Hardness (After Heat Treatment)58 – 64 HRC
Tensile Strength950 – 1200 MPa
Modulus of Elasticity210 GPa
en_USEnglish