4130 vs 4140 steel: let’s compare 4130 steel and AISI 4140 steel, drawing directly. Both are classified as medium-carbon, low-alloy steels and belong to the chromium-molybdenum alloy steel family.

Chemical Composition
4130 vs 4140 steel: composition comparison
| Element | AISI 4130 (wt%) | AISI 4140 (wt%) | Notes |
| Carbon | 0.28-0.33 | 0.38-0.43 | Higher carbon content in 4140 |
| Manganese | 0.40-0.60 | 0.75-1.00 | Higher manganese content in 4140 |
| Silicon | 0.20-0.35 | 0.20-0.35 | |
| Chromium | 0.80-1.10 | 0.80-1.10 | |
| Molybdenum | 0.15-0.25 | 0.15-0.25 |
Mechanical Properties
4130 vs 4140 steel: properties comparison. The mechanical properties are highly dependent on the heat treatment applied and the material’s section size. The data in this section is directly quoted from ASM International. (1991). ASM Handbook, Volume 4: Heat Treating (pp. 500-503). ASM International.
Typical mechanical properties of heat-treated 4130 steel.
| Tempering temperature | Tensile strength | Yield strength | Elongation in 50 mm (2 in.), % | Reduction in area, % | Hardness, HB | Izod impact energy | ||||
| °C | °F | MPa | ksi | MPa | ksi | |||||
| Water quenched and tempered. 25 mm (1 in.) diam round bars quenched from 845 to 870 °C (1550 to 1600 °F). | ||||||||||
| 205 | 400 | 1765 | 256 | 1765 | 1520 | 10 | 33 | 475 | 18 | 13 |
| 260 | 500 | 1670 | 242 | 1670 | 1430 | 11.5 | 37 | 455 | 14 | 10 |
| 315 | 600 | 1570 | 228 | 1570 | 1340 | 13 | 41 | 425 | 14 | 10 |
| 370 | 700 | 1475 | 214 | 1475 | 1250 | 15 | 45 | 400 | 20 | 15 |
| 425 | 800 | 1380 | 200 | 1380 | 1170 | 16.5 | 49 | 375 | 34 | 25 |
| 540 | 1000 | 1170 | 170 | 1170 | 1000 | 20 | 56 | 325 | 81 | 60 |
| 650 | 1200 | 965 | 140 | 965 | 830 | 22 | 63 | 270 | 135 | 100 |
| Oil quenched and tempered. 25 mm (1 in.) diam round bars quenched from 860 °C (1575 °F). | ||||||||||
| 205 | 400 | 1550 | 225 | 1340 | 195 | 11 | 38 | 450 | / | / |
| 260 | 500 | 1500 | 218 | 1275 | 185 | 11.5 | 40 | 440 | / | / |
| 315 | 600 | 1420 | 206 | 1210 | 175 | 12.5 | 43 | 418 | / | / |
| 370 | 700 | 1320 | 192 | 1120 | 162 | 14.5 | 48 | 385 | / | / |
| 425 | 800 | 1230 | 178 | 1030 | 150 | 16.5 | 54 | 360 | / | / |
| 540 | 1000 | 1030 | 150 | 840 | 122 | 20 | 60 | 305 | / | / |
| 650 | 1200 | 830 | 120 | 670 | 97 | 24 | 67 | 250 | / | / |
Effects of mass on typical properties of heat-treated 4130 steel
| Bar size (mm) | Bar size (in.) | Tensile strength (MPa) | Tensile strength (ksi) | Yield strength (MPa) | Yield strength (ksi) | Elongation in 50 mm (2 in.), % | Reduction in area, % | Surface hardness, HB |
| 25 | 1 | 1040 | 151 | 880 | 128 | 18 | 55 | 307 |
| 50 | 2 | 740 | 107 | 570 | 83 | 20 | 58 | 223 |
| 75 | 3 | 710 | 103 | 540 | 78 | 22 | 60 | 217 |
Note: Round bars oil quenched from 845 °C (1550 °F) and tempered at 540 °C (1000 °F); 12.83 mm (0.505 in.) diam tensile
Typical mechanical properties of heat-treated 4140 steel
| Tempering temperature (°C) | Tempering temperature (°F) | Tensile strength (MPa) | Tensile strength (ksi) | Yield strength (MPa) | Yield strength (ksi) | Elongation in 50 mm (2 in.), % | Reduction in area, % | Hardness, HB | Izod impact energy (J) | Izod impact energy (ft·lb) |
| 205 | 400 | 1965 | 285 | 1740 | 252 | 11 | 42 | 578 | 15 | 11 |
| 260 | 500 | 1860 | 270 | 1650 | 240 | 11 | 44 | 534 | 11 | 8 |
| 315 | 600 | 1720 | 250 | 1570 | 228 | 11.5 | 46 | 495 | 9 | 7 |
| 370 | 700 | 1590 | 231 | 1460 | 212 | 12.5 | 48 | 461 | 15 | 11 |
| 425 | 800 | 1450 | 210 | 1340 | 195 | 15 | 50 | 429 | 28 | 21 |
| 480 | 900 | 1300 | 188 | 1210 | 175 | 16 | 52 | 388 | 46 | 34 |
| 540 | 1000 | 1150 | 167 | 1050 | 152 | 17.5 | 55 | 341 | 65 | 48 |
| 595 | 1100 | 1020 | 148 | 910 | 132 | 19 | 58 | 311 | 93 | 69 |
| 650 | 1200 | 900 | 130 | 790 | 114 | 21 | 61 | 277 | 112 | 83 |
| 705 | 1300 | 810 | 117 | 690 | 100 | 23 | 65 | 235 | 136 | 100 |
Effects of mass on typical properties of heat-treated 4140 steel
| Diameter of bar (mm) | Diameter of bar (in.) | Tensile strength (MPa) | Tensile strength (ksi) | Yield strength (MPa) | Yield strength (ksi) | Elongation in 50 mm (2 in.), % | Reduction in area, % | Surface hardness, HB |
| 25 | 1 | 1140 | 165 | 985 | 143 | 15 | 50 | 335 |
| 50 | 2 | 920 | 133 | 750 | 109 | 18 | 55 | 202 |
| 75 | 3 | 860 | 125 | 655 | 95 | 19 | 55 | 293 |
Note: Round bars oil quenched from 845 °C (1550 °F) and tempered at 540 °C (1000 °F); 12.83 mm (0.505 in.) diam tensile specimens cut from center of 25 mm diam bars and from midradius of 50 and 75 mm diam bars

Heat Treatment Procedures
4140 Heat Treatment
- Normalizing: Heat to 870 to 925 °C (1600 to 1700 °F) and hold for a minimum of 1 hour or 15 to 20 minutes per 25 mm (1 in.) of maximum section thickness; air cool. Tempering at 480 °C (900 °F) or above is often performed after normalizing to decrease yield strength.
- Annealing: Heat to 830 to 870 °C (1525 to 1600 °F) and hold for a period dependent on section thickness or furnace load; furnace cool at about 15 °C/h (30 °F/h) to 480 °C (900 °F) and then air cool.
- Quenching: It’s a water-hardening alloy steel.
4130 heat treatment
- Normalizing: Heat to 845 to 925 °C (1550 to 1700 °F) and hold for 1-hour minimum or 15 to 20 minutes per 25 mm (1 in.) of maximum section thickness; air cool.
- Annealing: Heat to 830 to 870 °C (1525 to 1600 °F) and hold for a period dependent on section thickness or furnace load; furnace cool at about 15 °C/h (30 °F/h) to 480 °C (900 °F) and then air cool.
- Quenching: Oil-quenched from 855 °C (1575 °F) or 845 °C (1550 °F).
- Tempering: Has a simple tempering cycle, with 350°F (175 °C) commonly used. To avoid blue brittleness, 4140 is usually not tempered between 230 and 370 °C (450 to 700 °F). Tempering temperature and time depend on the desired hardness.
Summary
Based on their characteristics and usage experience, here is a summary of the differences between 4140 and 4340 steel.
4140, with its higher carbon and manganese content, generally offers greater hardenability and higher strength compared to 4130. This makes 4140 suitable for applications requiring higher strength in heavier sections, assuming appropriate heat treatment. 4140 has better hardenability, but requires a milder quenching process than 4130 to achieve the same quenching effect on parts with the same geometry. 4140 has a certain probability of cracking and deformation due to excessive cooling speed during the quenching process. When quenching 4140, it is essential to control the quenching parameters strictly.
For thin sections, a plain carbon steel might suffice, while for heavier sections requiring hardening, 4140 would be needed. However, selecting a more expensive alloy like 4340 (which has even higher hardenability due to Nickel-Chromium-Molybdenum) might be unnecessary if 4140 is adequate. Generally, steels with Cr-Ni-Mo are most expensive, followed by Cr-Mo, then Cr-V.