{"id":9929,"date":"2025-08-27T12:10:41","date_gmt":"2025-08-27T04:10:41","guid":{"rendered":"https:\/\/aobosteel.com\/"},"modified":"2026-10-14T14:00:08","modified_gmt":"2026-10-14T06:00:08","slug":"cr5mo1v-tool-steel","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/cr5mo1v-tool-steel\/","title":{"rendered":"Fornecedor de a\u00e7o ferramenta para trabalho a frio Cr5Mo1V"},"content":{"rendered":"\n<style id=\"aobo-steel-rebuild\" data-noptimize=\"1\">\n\/* Rebuilt tool-steel page: banner is full-bleed, the body keeps the site's normal\n   content width. All layout rules live in this page, so a missing external\n   stylesheet can no longer collapse the page. *\/\n.ads2 *, .ads2 *::before, .ads2 *::after { box-sizing: border-box; }\n.ads2 { font-size: 16px; line-height: 1.75; color: #2b2b2b; }\n.ads2-hero { position: relative; width: 100vw !important; max-width: 100vw !important;\n  margin-left: calc(50% - 50vw) !important; margin-right: 0 !important;\n  min-height: 430px; display: flex; align-items: center; overflow: hidden; background: #1d1d1d; }\n.ads2-hero-img { position: absolute; inset: 0; width: 100%; height: 100%; object-fit: cover; }\n.ads2-hero-ov { position: absolute; inset: 0; background: #4e4b40; opacity: .5; }\n.ads2-hero-scrim { position: absolute; inset: 0;\n  background: linear-gradient(90deg, rgba(0,0,0,.42) 0%, rgba(0,0,0,.32) 45%, rgba(0,0,0,.16) 78%, rgba(0,0,0,.04) 100%); }\n.ads2-hero-in { position: relative; width: 100%; max-width: 1200px; margin: 0 auto; padding: 56px 24px; color: #fff; }\n.ads2-crumb, .ads2-crumb a, .ads2-crumb h6, .ads2-crumb mark { color: #dfe6ef !important; font-size: 13px;\n  text-decoration: none; letter-spacing: .2px; }\n.ads2-crumb h6 { display: inline; font-weight: 400; margin: 0; }\n.ads2-crumb a:hover { color: #fff !important; text-decoration: underline; }\n.ads2-tag { margin: 10px 0 6px; color: #eef1f5 !important; font-size: 14px; text-shadow: 0 1px 6px rgba(0,0,0,.8); }\n.ads2-h1 { margin: 0 0 12px; font-size: 40px; line-height: 1.2; font-weight: 800; color: #fff !important;\n  letter-spacing: -.2px; max-width: 900px; text-shadow: 0 2px 14px rgba(0,0,0,.85), 0 0 4px rgba(0,0,0,.55); }\n.ads2-sub { margin: 0 0 20px; font-size: 17px; color: #fff !important; text-shadow: 0 1px 8px rgba(0,0,0,.9), 0 0 3px rgba(0,0,0,.6); }\n.ads2-checks { list-style: none; margin: 0 0 26px; padding: 0; display: flex; flex-wrap: wrap; gap: 8px 22px; }\n.ads2-checks li { position: relative; margin: 0; padding-left: 20px; font-size: 15px; color: #fff !important;\n  text-shadow: 0 1px 6px rgba(0,0,0,.85); }\n.ads2-checks li::before { content: \"\\2713\"; position: absolute; left: 0; top: 0; color: #4ade80; font-weight: 700; }\n.ads2-cta { margin: 24px 0 6px; text-align: center; }\n.ads2-hero .ads2-cta { text-align: left; margin-top: 26px; }\n.ads2-btn { display: inline-block; background: #074fd0; color: #fff !important; font-weight: 400;\n  font-size: 16px; line-height: 16px; padding: 14px 30px; border-radius: 100px;\n  text-decoration: none !important; cursor: pointer; }\n.ads2-btn:hover { background: #063c9e; color: #fff !important; }\n.ads2-body { max-width: 1200px; margin: 0 auto; padding: 48px 24px 64px; }\n.ads2-sec { margin: 0 0 54px; }\n.ads2-sec:last-child { margin-bottom: 0; }\n.ads2 h2 { font-size: 27px; line-height: 1.3; color: #062a5a; font-weight: 700; margin: 0 0 20px;\n  padding-bottom: 12px; border-bottom: 1px solid #e6eaef; }\n.ads2 h3 { font-size: 21px; color: #062a5a; margin: 28px 0 12px; }\n.ads2 h4 { font-size: 18px; color: #062a5a; margin: 22px 0 10px; }\n.ads2 p { margin: 0 0 16px; }\n.ads2 a { color: #005fcf; text-decoration: none; }\n.ads2 a:hover { text-decoration: underline; }\n.ads2 ul, .ads2 ol { margin: 0 0 18px; padding-left: 22px; }\n.ads2 li { margin: 0 0 8px; }\n.ads2-cols2 { display: grid; grid-template-columns: 1fr 1fr; gap: 8px 40px; }\n.ads2-cols2 ul { margin-bottom: 0; }\n.ads2-row { display: grid; grid-template-columns: 1.05fr .95fr; gap: 36px; align-items: center; }\n.ads2-row-flip .ads2-col-i { order: -1; }\n.ads2-row .ads2-col-t > *:last-child { margin-bottom: 0; }\n.ads2-row .ads2-cta { margin-top: 16px; }\n.ads2-fig { margin: 0 0 22px; }\n.ads2-fig img { width: 100%; height: auto; display: block; }\n.ads2-gal { display: grid; grid-template-columns: repeat(3, 1fr); gap: 16px; margin: 0 0 22px; }\n.ads2-gal .ads2-fig { margin: 0; }\n.ads2-row .ads2-fig { margin: 0; }\n.ads2-tw { margin: 0 0 22px; overflow-x: auto; }\n.ads2-t { width: 100%; border-collapse: collapse; font-size: 15px; }\n.ads2-t td, .ads2-t th { border: 1px solid #e3e7ec; padding: 11px 14px; vertical-align: top; text-align: left; }\n.ads2-t.kv td:first-child { background: #f6f8fa; font-weight: 600; color: #062a5a; width: 34%; }\n.ads2-t.data { font-size: 14.5px; }\n.ads2-t.data td, .ads2-t.data th { padding: 9px 11px; }\n.ads2-t.data thead th, .ads2-t.data tr:first-child td { background: #eef3f9; font-weight: 700; color: #062a5a; }\n.ads2-t.data tbody tr:nth-child(odd) td { background: #fbfcfd; }\n@media (max-width: 1000px) {\n  .ads2-row { grid-template-columns: 1fr; gap: 22px; }\n  .ads2-row-flip .ads2-col-i { order: 0; }\n  .ads2-cols2 { grid-template-columns: 1fr; }\n  .ads2-h1 { font-size: 30px; }\n  .ads2-hero { min-height: 340px; }\n}\n@media (max-width: 700px) {\n  .ads2-gal { grid-template-columns: 1fr; }\n  .ads2-body { padding: 32px 18px 44px; }\n  .ads2-t { font-size: 14px; }\n  .ads2-t td, .ads2-t th { padding: 9px 10px; }\n  .ads2-t.kv td:first-child { width: 42%; }\n  .ads2-tw { -webkit-overflow-scrolling: touch; }\n}\n@media (max-width: 640px) {\n  .ads2-hero-in { padding: 34px 18px 38px; }\n  .ads2-h1 { font-size: 25px; }\n  .ads2 h2 { font-size: 22px; }\n  .ads2-tag { font-size: 13px; }\n  .ads2-sub { font-size: 15px; }\n  .ads2-checks { gap: 6px 16px; }\n  .ads2-checks li { font-size: 14px; }\n  .ads2-btn { padding: 12px 24px; font-size: 15px; }\n  .ads2-sec { margin-bottom: 40px; }\n}\n<\/style>\n<div class=\"ads2\">\n<section class=\"ads2-hero\">\n  <img class=\"ads2-hero-img\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/05\/banner3.webp\" sizes=\"100vw\" alt=\"Bulk tool steel bar stock in the Aobo Steel warehouse\" loading=\"eager\" decoding=\"async\">\n  <div class=\"ads2-hero-ov\"><\/div>\n  <div class=\"ads2-hero-scrim\"><\/div>\n  <div class=\"ads2-hero-in\">\n    <h1 class=\"ads2-h1\">Cr5Mo1V Cold Work Tool Steel<\/h1>\n    <p class=\"ads2-tag\"><em>Aobo Steel- Trusted Global Tool Steel Supplier<\/em><\/p>\n    <div class=\"ads2-cta popmake-16052\"><a class=\"ads2-btn\" href=\"#\">Send Inquiry Now<\/a><\/div>\n  <\/div>\n<\/section>\n<div class=\"ads2-body\">\n<section class=\"ads2-sec\">\n<p>Cr5Mo1V is a medium alloy air-hardening cold work tool steel, also classified as a high carbon medium chromium tool steel. <span style=\"box-sizing: border-box; margin: 0px; padding: 0px;\">It is recognized by the unified digital code T20503 and equivalent to American\u00a0<a href=\"https:\/\/aobosteel.com\/a2-tool-steel\/\" target=\"_blank\"><mark style=\"background-color:rgba(0, 0, 0, 0);color:#0693e3\" class=\"has-inline-color\">A2 steel<\/mark><\/a>, JIS SKD12 in Japan, and DIN 1.2363 in German<\/span>y. It is a versatile material, particularly suitable for applications that demand both good wear resistance and good toughness.<\/p>\n<\/section>\n<section class=\"ads2-sec\">\n<h2>1. Chemical Composition(GB\/T 1299\u20142000)<\/h2>\n<div class=\"ads2-tw\"><table class=\"ads2-t data\"><thead><tr><th>C<\/th><th>Si<\/th><th>Mn<\/th><th>Cr<\/th><th>Mo<\/th><th>V<\/th><th>P<\/th><th>S<\/th><\/tr><\/thead><tbody><tr><td>0.95 &#8211; 1.05%<\/td><td>\u22640.50%<\/td><td>\u22641.00%<\/td><td>4.75 &#8211; 5.50%<\/td><td>0.90 &#8211; 1.40%<\/td><td>0.15 &#8211; 0.50%<\/td><td>\u22640.030%<\/td><td>\u22640.030%<\/td><\/tr><\/tbody><\/table><\/div>\n<\/section>\n<section class=\"ads2-sec\">\n<h2>2. Physical Properties of Cr5Mo1V Steel<\/h2>\n<p><strong>2.1 Cr5Mo1V Steel Critical Temperature<\/strong><\/p>\n<div class=\"ads2-tw\"><table class=\"ads2-t data\"><thead><tr><td><strong>Critical Point<\/strong><\/td><td><strong>Ac\u2081<\/strong><\/td><td><strong>Accm<\/strong><\/td><td><strong>Ms<\/strong><\/td><\/tr><\/thead><tbody><tr><td>Temperature\/\u00b0C<\/td><td>795<\/td><td>\u2014<\/td><td>168<\/td><\/tr><\/tbody><\/table><\/div>\n<p><strong>2.2 Cr5Mo1V Steel Linear Expansion Coefficient<\/strong><\/p>\n<div class=\"ads2-tw\"><table class=\"ads2-t data\"><thead><tr><td><strong>Temperature \/\u00b0C<\/strong><\/td><td><strong>20 ~ 100<\/strong><\/td><td><strong>20 ~ 300<\/strong><\/td><td><strong>20 ~ 500<\/strong><\/td><td><strong>20 ~ 700<\/strong><\/td><\/tr><\/thead><tbody><tr><td>Linear Expansion Coefficient \u03b1\/ \u00d710\u207b\u2076\u00b0C\u207b\u00b9<\/td><td>8.2<\/td><td>11.3<\/td><td>12.4<\/td><td>12.9<\/td><\/tr><\/tbody><\/table><\/div>\n<p><strong>2.3 Cr5Mo1V Steel Other Physical Properties<\/strong><\/p>\n<div class=\"ads2-tw\"><table class=\"ads2-t data\"><thead><tr><td><strong>Density \/ (g\/cm\u00b3)<\/strong><\/td><td><strong>Modulus of Elasticity E (Room Temperature) \/MPa<\/strong><\/td><td><strong>Specific Heat Capacity c\u209a\/ [J\/(kg\u00b7K)]<\/strong><\/td><\/tr><\/thead><tbody><tr><td>7.84<\/td><td>203000<\/td><td>460.55<\/td><\/tr><\/tbody><\/table><\/div>\n<\/section>\n<section class=\"ads2-sec\">\n<h2>3. <strong>Cr5Mo1V Steel Forging Process Specification<\/strong><\/h2>\n<div class=\"ads2-tw\"><table class=\"ads2-t data\"><thead><tr><td><strong>Item<\/strong><\/td><td><strong>Heating Temperature\/\u00b0C<\/strong><\/td><td><strong>Initial Forging Temperature\/\u00b0C<\/strong><\/td><td><strong>Final Forging Temperature\/\u00b0C<\/strong><\/td><td><strong>Cooling Method<\/strong><\/td><\/tr><\/thead><tbody><tr><td>Steel Ingot<\/td><td>1100 ~ 1150<\/td><td>1050 ~ 1100<\/td><td>850 ~ 900<\/td><td>High-temperature annealing, pit cooling, or sand cooling<\/td><\/tr><tr><td>Steel Billet<\/td><td>1050 ~ 1100<\/td><td>1000 ~ 1050<\/td><td>850 ~ 900<\/td><td>Pit cooling or sand cooling<\/td><\/tr><\/tbody><\/table><\/div>\n\n\n<div class=\"wp-block-columns is-layout-flex wp-container-core-columns-is-layout-7387b849 wp-block-columns-is-layout-flex\">\n<div class=\"wp-block-column is-layout-flow wp-block-column-is-layout-flow\">\n<figure class=\"wp-block-image aligncenter size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"722\" height=\"722\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif\" alt=\"Cr5Mo1V\" class=\"wp-image-9931\" srcset=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif 722w, https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V-300x300.avif 300w, https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V-150x150.avif 150w, https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V-12x12.avif 12w\" sizes=\"auto, (max-width: 722px) 100vw, 722px\" \/><figcaption class=\"wp-element-caption\">Cr5Mo1V steel<\/figcaption><\/figure>\n<\/div>\n\n\n\n<div class=\"wp-block-column is-layout-flow wp-block-column-is-layout-flow\">\n<p class=\"wp-block-paragraph\"><strong>Please complete the following contact form to receive the best Cr5Mo1V steel quotation.<\/strong><\/p>\n\n\n\n<div class=\"wp-block-contact-form-7-contact-form-selector\">\n<div class=\"wpcf7 no-js\" id=\"wpcf7-f16042-o1\" lang=\"en-US\" dir=\"ltr\" data-wpcf7-id=\"16042\">\n<div class=\"screen-reader-response\"><p role=\"status\" aria-live=\"polite\" aria-atomic=\"true\"><\/p> <ul><\/ul><\/div>\n<form action=\"\/pt\/wp-json\/wp\/v2\/pages\/9929#wpcf7-f16042-o1\" method=\"post\" class=\"wpcf7-form init\" aria-label=\"Contact form\" novalidate=\"novalidate\" data-status=\"init\">\n<fieldset class=\"hidden-fields-container\"><input type=\"hidden\" name=\"_wpcf7\" value=\"16042\" \/><input type=\"hidden\" name=\"_wpcf7_version\" value=\"6.2.6\" \/><input type=\"hidden\" name=\"_wpcf7_locale\" value=\"en_US\" \/><input type=\"hidden\" name=\"_wpcf7_unit_tag\" value=\"wpcf7-f16042-o1\" \/><input type=\"hidden\" name=\"_wpcf7_container_post\" value=\"0\" \/><input type=\"hidden\" name=\"_wpcf7_posted_data_hash\" value=\"\" \/>\n<\/fieldset>\n<div class=\"wpcf7-turnstile cf-turnstile\" data-sitekey=\"0x4AAAAAAFMY32JbOfIdWijB\" data-response-field-name=\"_wpcf7_turnstile_response\"><\/div>\n\n<p><span class=\"wpcf7-form-control-wrap\" data-name=\"your-name\"><input size=\"40\" maxlength=\"400\" class=\"wpcf7-form-control wpcf7-text wpcf7-validates-as-required\" autocomplete=\"name\" aria-required=\"true\" aria-invalid=\"false\" placeholder=\"Your Name *\" value=\"\" type=\"text\" name=\"your-name\" \/><\/span>\n<\/p>\n<p><span class=\"wpcf7-form-control-wrap\" data-name=\"your-email\"><input size=\"40\" maxlength=\"400\" class=\"wpcf7-form-control wpcf7-email wpcf7-validates-as-required wpcf7-text wpcf7-validates-as-email\" autocomplete=\"email\" aria-required=\"true\" aria-invalid=\"false\" placeholder=\"Email *\" value=\"\" type=\"email\" name=\"your-email\" \/><\/span>\n<\/p>\n<p><span class=\"wpcf7-form-control-wrap\" data-name=\"your-message\"><textarea cols=\"40\" rows=\"4\" maxlength=\"2000\" class=\"wpcf7-form-control wpcf7-textarea wpcf7-validates-as-required\" aria-required=\"true\" aria-invalid=\"false\" placeholder=\"Message *\" name=\"your-message\"><\/textarea><\/span>\n<\/p>\n<p><input class=\"wpcf7-form-control wpcf7-submit has-spinner\" type=\"submit\" value=\"Send Inquiry\" \/>\n<\/p><p style=\"display: none !important;\" class=\"akismet-fields-container\" data-prefix=\"_wpcf7_ak_\"><label>&#916;<textarea name=\"_wpcf7_ak_hp_textarea\" cols=\"45\" rows=\"8\" maxlength=\"100\"><\/textarea><\/label><input type=\"hidden\" id=\"ak_js_1\" name=\"_wpcf7_ak_js\" value=\"141\"\/><script>\ndocument.getElementById( \"ak_js_1\" ).setAttribute( \"value\", ( new Date() ).getTime() );\n<\/script>\n<\/p><input type='hidden' class='wpcf7-pum' value='{\"closepopup\":false,\"closedelay\":0,\"openpopup\":true,\"openpopup_id\":16052}' \/><div class=\"wpcf7-response-output\" aria-hidden=\"true\"><\/div>\n<\/form>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n\n\n\n<\/section>\n<section class=\"ads2-sec\">\n<h2>4. Heat treatment of Cr5Mo1V Steel<\/h2>\n<p><strong>4.1 Preheating<\/strong><\/p>\n<div class=\"ads2-tw\"><table class=\"ads2-t kv\"><tbody><tr><td><strong>Preliminary Heat Treatment Plan<\/strong><\/td><td><strong>Process Parameters<\/strong><\/td><\/tr><tr><td>General Annealing after Forging<\/td><td>Heating temperature is 840 ~ 870\u00b0C, hold for 2 ~ 3h; furnace cool to below 550\u00b0C then air cool, hardness \u2264248HBW<\/td><\/tr><tr><td>Isothermal Annealing after Forging<\/td><td>Heating temperature is 830 ~ 850\u00b0C, hold for 2h; isothermal temperature is 710 ~ 730\u00b0C, hold for 2 ~ 4h, furnace cool to 500\u00b0C then air cool or furnace cool to room temperature, hardness after annealing \u2264248HBW<\/td><\/tr><\/tbody><\/table><\/div>\n<p><strong>4.2 Quenching<\/strong><\/p>\n<p>\u2460 Recommended Quenching Process Specification<\/p>\n<div class=\"ads2-tw\"><table class=\"ads2-t data\"><thead><tr><td><strong>Plan<\/strong><\/td><td><strong>First Preheating Temperature\/\u00b0C<\/strong><\/td><td><strong>Second Preheating Temperature\/\u00b0C<\/strong><\/td><td><strong>Quenching Temperature\/\u00b0C<\/strong><\/td><td><strong>Cooling<\/strong><\/td><td><strong>Hardness HRC<\/strong><\/td><\/tr><\/thead><tbody><tr><td>I<\/td><td>300 ~ 400<\/td><td>800 ~ 850<\/td><td>940 ~ 960<\/td><td>Air cooling or oil cooling<\/td><td>62 ~ 63<\/td><\/tr><tr><td>II<\/td><td>300 ~ 400<\/td><td>800 ~ 850<\/td><td>980 ~ 1010<\/td><td>Air cooling or oil cooling<\/td><td>62 ~ 65<\/td><\/tr><\/tbody><\/table><\/div>\n<p>\u2461 Effect of Quenching Temperature on Hardness<\/p>\n<div class=\"ads2-tw\"><table class=\"ads2-t data\"><thead><tr><td><strong>Quenching Temperature\/\u00b0C<\/strong><\/td><td><strong>875<\/strong><\/td><td><strong>900<\/strong><\/td><td><strong>960<\/strong><\/td><td><strong>980<\/strong><\/td><td><strong>1020<\/strong><\/td><td><strong>1050<\/strong><\/td><\/tr><\/thead><tbody><tr><td>Hardness HRC<\/td><td>46.5<\/td><td>54<\/td><td>64.5<\/td><td>64.5<\/td><td>63<\/td><td>58<\/td><\/tr><\/tbody><\/table><\/div>\n<p><strong>4.3 Tempering<\/strong><\/p>\n<p>\u2460 Recommended Tempering Process Specification<\/p>\n<div class=\"ads2-tw\"><table class=\"ads2-t data\"><thead><tr><td><strong>Quenching Plan<\/strong><\/td><td><strong>Tempering Temperature\/\u00b0C<\/strong><\/td><td><strong>Number of Tempers<\/strong><\/td><td><strong>Hardness HRC<\/strong><\/td><\/tr><\/thead><tbody><tr><td>I<\/td><td>180 ~ 220<\/td><td>1<\/td><td>60 ~ 64<\/td><\/tr><tr><td>II<\/td><td>510 ~ 520<\/td><td>2<\/td><td>57 ~ 60<\/td><\/tr><\/tbody><\/table><\/div>\n<p>\u2461 Effect of Tempering Temperature on Hardness<\/p>\n<div class=\"ads2-tw\"><table class=\"ads2-t data\"><thead><tr><td>Quenching Condition<\/td><td>Tempering Temperature\/\u00b0C<\/td><td>100<\/td><td>200<\/td><td>300<\/td><td>400<\/td><td>450<\/td><td>500<\/td><td>520<\/td><td>580<\/td><\/tr><\/thead><tbody><tr><td>954\u00b0C Quenching<\/td><td>Hardness HRC<\/td><td>64.5<\/td><td>62<\/td><td>58<\/td><td>57<\/td><td>56<\/td><td>59<\/td><td>56<\/td><td>51<\/td><\/tr><tr><td>982\u00b0C Quenching<\/td><td>Hardness HRC<\/td><td>65<\/td><td>62<\/td><td>58<\/td><td>58<\/td><td>56<\/td><td>58<\/td><td>57<\/td><td>51.5<\/td><\/tr><\/tbody><\/table><\/div>\n<\/section>\n<section class=\"ads2-sec\">\n<h2>5. Mechanical Properties<\/h2>\n<p>Cr5Mo1V steel is a free-hardening steel exhibiting high free-hardening properties. It features relatively low quenching distortion, high hardness, excellent wear resistance, and moderate toughness, delivering outstanding overall mechanical properties.<\/p>\n<p><strong>Mechanical Properties of Cr5Mo1V Steel after Tempering<\/strong><\/p>\n<div class=\"ads2-tw\"><table class=\"ads2-t data\"><thead><tr><td><strong>Tempering Temperature\/\u00b0C<\/strong><\/td><td><strong>Hardness HRC<\/strong><\/td><td><strong>Tensile Strength\/MPa<\/strong><\/td><td><strong>Yield Strength\/MPa<\/strong><\/td><td><strong>Elongation (%)<\/strong><\/td><td><strong>Reduction of Area (%)<\/strong><\/td><\/tr><\/thead><tbody><tr><td>530<\/td><td>54.1<\/td><td>1849<\/td><td>\u2014<\/td><td>\u2014<\/td><td>\u2014<\/td><\/tr><tr><td>593<\/td><td>46.7<\/td><td>1596<\/td><td>576<\/td><td>5.0<\/td><td>13.9<\/td><\/tr><\/tbody><\/table><\/div>\n<p>Note: 980\u00b0C air cooling.<\/p>\n<\/section>\n<section class=\"ads2-sec\">\n<h2>6. Applications<\/h2>\n<p>Cr5Mo1V steel exhibits excellent comprehensive mechanical properties, making it particularly suitable for manufacturing tools and dies that require both high wear resistance and good toughness, as well as dimensional stability. Examples include rollers, punches, blanking dies, forming dies, rolling dies, wire drawing dies, and thread rolling dies. It is also used for certain types of shear blades.<\/p>\n<div class=\"ads2-gal\"><figure class=\"ads2-fig\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif\" alt=\"Cr5Mo1V\"><figcaption>Cr5Mo1V steel<\/figcaption><\/figure><figure class=\"ads2-fig\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/03\/A2-MATERIAL.webp\" alt=\"A2 tool steel\"><figcaption>A2 tool steel<\/figcaption><\/figure><figure class=\"ads2-fig\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/06\/A2-STEEL.webp\" alt=\"A2 STEEL\"><figcaption>A2 tool steel plates<\/figcaption><\/figure><\/div>\n<div class=\"ads2-cta popmake-16052\"><a class=\"ads2-btn\" href=\"#\">Open RFQ Form<\/a><\/div>\n<\/section>\n<\/div>\n<\/div>\n\n","protected":false},"excerpt":{"rendered":"<p>Cr5Mo1V Cold Work Tool Steel Aobo Steel- Trusted Global Tool Steel Supplier Send Inquiry Now Cr5Mo1V is a medium alloy air-hardening cold work tool steel, also classified as a high carbon medium chromium tool steel. It is recognized by the unified digital code T20503 and equivalent to American\u00a0A2 steel, JIS SKD12 in Japan, and DIN [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":9931,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"disabled","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-9929","page","type-page","status-publish","has-post-thumbnail","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Cr5Mo1V Cold Work Tool Steel Supplier - AoboSteel<\/title>\n<meta name=\"description\" content=\"Discover the unique features of Cr5Mo1V, a high carbon medium chromium tool steel ideal for cold work environments.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/cr5mo1v-tool-steel\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Cr5Mo1V Cold Work Tool Steel Supplier\" \/>\n<meta property=\"og:description\" content=\"Discover the unique features of Cr5Mo1V, a high carbon medium chromium tool steel ideal for cold work environments.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/cr5mo1v-tool-steel\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-14T06:00:08+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif\" \/>\n\t<meta property=\"og:image:width\" content=\"722\" \/>\n\t<meta property=\"og:image:height\" content=\"722\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/png\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"4 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Cr5Mo1V Cold Work Tool Steel Supplier\",\"datePublished\":\"2025-08-27T04:10:41+00:00\",\"dateModified\":\"2026-10-14T06:00:08+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/\"},\"wordCount\":507,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/08\\\/Cr5Mo1V.avif\",\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/\",\"name\":\"Cr5Mo1V Cold Work Tool Steel Supplier - AoboSteel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/08\\\/Cr5Mo1V.avif\",\"datePublished\":\"2025-08-27T04:10:41+00:00\",\"dateModified\":\"2026-10-14T06:00:08+00:00\",\"description\":\"Discover the unique features of Cr5Mo1V, a high carbon medium chromium tool steel ideal for cold work environments.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/08\\\/Cr5Mo1V.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/08\\\/Cr5Mo1V.avif\",\"width\":722,\"height\":722,\"caption\":\"Cr5Mo1V steel\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/cr5mo1v-tool-steel\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Cr5Mo1V Cold Work Tool Steel Supplier\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Fornecedor de a\u00e7o ferramenta para trabalho a frio Cr5Mo1V - AoboSteel","description":"Descubra as caracter\u00edsticas exclusivas do Cr5Mo1V, um a\u00e7o para ferramentas com alto teor de carbono e m\u00e9dio cromo, ideal para ambientes de trabalho a frio.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/cr5mo1v-tool-steel\/","og_locale":"pt_BR","og_type":"article","og_title":"Cr5Mo1V Cold Work Tool Steel Supplier","og_description":"Discover the unique features of Cr5Mo1V, a high carbon medium chromium tool steel ideal for cold work environments.","og_url":"https:\/\/aobosteel.com\/pt\/cr5mo1v-tool-steel\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-14T06:00:08+00:00","og_image":[{"width":722,"height":722,"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif","type":"image\/png"}],"twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"4 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Cr5Mo1V Cold Work Tool Steel Supplier","datePublished":"2025-08-27T04:10:41+00:00","dateModified":"2026-10-14T06:00:08+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/"},"wordCount":507,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif","inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/","url":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/","name":"Fornecedor de a\u00e7o ferramenta para trabalho a frio Cr5Mo1V - AoboSteel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif","datePublished":"2025-08-27T04:10:41+00:00","dateModified":"2026-10-14T06:00:08+00:00","description":"Descubra as caracter\u00edsticas exclusivas do Cr5Mo1V, um a\u00e7o para ferramentas com alto teor de carbono e m\u00e9dio cromo, ideal para ambientes de trabalho a frio.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/"]}]},{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif","width":722,"height":722,"caption":"Cr5Mo1V steel"},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/cr5mo1v-tool-steel\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Cr5Mo1V Cold Work Tool Steel Supplier"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"thumbnail":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V-150x150.avif",150,150,true],"medium":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V-300x300.avif",300,300,true],"medium_large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"1536x1536":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"2048x2048":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"trp-custom-language-flag":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V-12x12.avif",12,12,true]},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Cr5Mo1V Cold Work Tool Steel Aobo Steel- Trusted Global Tool Steel Supplier Send Inquiry Now Cr5Mo1V is a medium alloy air-hardening cold work tool steel, also classified as a high carbon medium chromium tool steel. It is recognized by the unified digital code T20503 and equivalent to American\u00a0A2 steel, JIS SKD12 in Japan, and DIN&hellip;","rttpg_featured_image_url":{"full":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"landscape":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"portraits":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"thumbnail":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V-150x150.avif",150,150,true],"medium":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V-300x300.avif",300,300,true],"large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"1536x1536":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"2048x2048":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V.avif",722,722,false],"trp-custom-language-flag":["https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/08\/Cr5Mo1V-12x12.avif",12,12,true]},"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Cr5Mo1V Cold Work Tool Steel Aobo Steel- Trusted Global Tool Steel Supplier Send Inquiry Now Cr5Mo1V is a medium alloy air-hardening cold work tool steel, also classified as a high carbon medium chromium tool steel. It is recognized by the unified digital code T20503 and equivalent to American\u00a0A2 steel, JIS SKD12 in Japan, and DIN&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/9929","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=9929"}],"version-history":[{"count":4,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/9929\/revisions"}],"predecessor-version":[{"id":22241,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/9929\/revisions\/22241"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media\/9931"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=9929"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}