{"id":21450,"date":"2026-10-09T12:36:25","date_gmt":"2026-10-09T04:36:25","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=21450"},"modified":"2026-10-11T11:02:02","modified_gmt":"2026-10-11T03:02:02","slug":"thermal-fatigue-cracking-in-die-casting-dies","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/thermal-fatigue-cracking-in-die-casting-dies\/","title":{"rendered":"Trincas por fadiga t\u00e9rmica em moldes de fundi\u00e7\u00e3o sob press\u00e3o"},"content":{"rendered":"\n<style>\n\n:root{\n    --aobo-accent:#2563eb; --aobo-accent-dark:#1e1e2e; --aobo-blue:#0c56d0; --aobo-blue-dark:#073b91;\n    --aobo-text:#333; --aobo-muted:#888; --aobo-border:#e5e7eb; --aobo-border-dark:#ddd;\n    --aobo-stripe:#f7f7f9; --aobo-hover:#e8f0fe; --aobo-radius:8px; --aobo-radius-sm:6px;\n    --aobo-orange:#f59e0b; --aobo-fill:#e9ecef;\n  }\n  *{box-sizing:border-box;}\n  html{-webkit-text-size-adjust:100%;}\n  body{margin:0;background:#fff;color:var(--aobo-text);\n    font-family:-apple-system,BlinkMacSystemFont,\"Segoe UI\",Roboto,\"Helvetica Neue\",Arial,sans-serif;\n    font-size:15px;line-height:1.6;}\n\n  \/* Root scope \u2014 WordPress theme guard *\/\n  .ts-props{color:var(--aobo-text);background:transparent;padding:0;box-sizing:border-box;line-height:1.6;}\n  .ts-props *{box-sizing:border-box;}\n  .ts-props button,.ts-props input[type=\"text\"]{\n    background:none !important;border:none !important;border-radius:0 !important;padding:0 !important;\n    margin:0 !important;font-size:inherit !important;font-weight:inherit !important;\n    letter-spacing:normal !important;text-transform:none !important;box-shadow:none !important;\n    line-height:inherit !important;text-decoration:none !important;}\n\n  .aobo-wrap{max-width:1160px;margin:0 auto;}\n\n  \/* Hero *\/\n  .ts-hero{background:#fff;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);overflow:hidden;}\n  .ts-hero-top{padding:1.5em;background:var(--aobo-stripe);border-bottom:1px solid var(--aobo-border);}\n  .ts-kicker{display:inline-flex;align-items:center;gap:6px;color:var(--aobo-accent);background:var(--aobo-hover);\n    border:1px solid var(--aobo-border);border-radius:var(--aobo-radius-sm);padding:4px 8px;\n    font-size:.85em;font-weight:600;margin-bottom:.8em;}\n  .ts-kicker span{width:6px;height:6px;background:var(--aobo-orange);border-radius:50%;display:inline-block;}\n  .ts-hero h1{margin:0;font-size:2rem;line-height:1.3;color:var(--aobo-text);text-align:center;}\n  .ts-hero-top p{margin:.6em auto 0;max-width:820px;font-size:.9em;line-height:1.6;color:var(--aobo-muted);text-align:center;}\n\n  \/* Tool area *\/\n  .ts-tool-area{padding:1.5em;}\n\n  \/* Legend *\/\n  .ts-legend{display:flex;flex-wrap:wrap;gap:8px;margin-bottom:1em;}\n  .ts-legend > span{display:inline-flex;align-items:center;gap:5px;font-size:.8em;color:var(--aobo-muted);\n    background:var(--aobo-stripe);border:1px solid var(--aobo-border);border-radius:var(--aobo-radius-sm);\n    padding:3px 8px;}\n  .ts-legend b{color:var(--aobo-text);font-weight:600;}\n  .ts-legend .ts-dot{width:9px;height:9px;border-radius:50%;background:var(--aobo-accent);display:inline-block;\n    padding:0;border:0;gap:0;}\n\n  \/* Controls *\/\n  .ts-controls{display:flex;flex-wrap:wrap;gap:10px;align-items:center;background:var(--aobo-stripe);\n    border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);padding:1em;margin-bottom:1.2em;}\n  .ts-search{flex:1 1 220px;max-width:340px;position:relative;}\n  .ts-props .ts-search input{width:100% !important;border:1px solid var(--aobo-border-dark) !important;\n    border-radius:var(--aobo-radius-sm) !important;padding:.5em .6em .5em 2em !important;\n    font-size:.92em !important;color:var(--aobo-text) !important;background:#fff !important;\n    outline:none !important;box-shadow:none !important;}\n  .ts-props .ts-search input:focus{border-color:var(--aobo-accent) !important;\n    box-shadow:0 0 0 2px rgba(37,99,235,.12) !important;}\n  .ts-search::before{content:\"\";position:absolute;left:.7em;top:50%;transform:translateY(-50%);\n    width:13px;height:13px;background:var(--aobo-muted);\n    -webkit-mask:url(\"data:image\/svg+xml;utf8,<svg xmlns='http:\/\/www.w3.org\/2000\/svg' viewBox='0 0 24 24' fill='none' stroke='black' stroke-width='2'><circle cx='11' cy='11' r='8'\/><path d='m21 21-4.3-4.3'\/><\/svg>\") center\/contain no-repeat;\n    mask:url(\"data:image\/svg+xml;utf8,<svg xmlns='http:\/\/www.w3.org\/2000\/svg' viewBox='0 0 24 24' fill='none' stroke='black' stroke-width='2'><circle cx='11' cy='11' r='8'\/><path d='m21 21-4.3-4.3'\/><\/svg>\") center\/contain no-repeat;}\n  .ts-chips{display:flex;flex-wrap:wrap;gap:6px;}\n  .ts-props .ts-chip{border:1px solid var(--aobo-border-dark) !important;background:#fff !important;\n    color:var(--aobo-text) !important;border-radius:999px !important;padding:.4em .9em !important;\n    font-size:.8em !important;font-weight:600 !important;cursor:pointer !important;transition:all .15s !important;}\n  .ts-props .ts-chip:hover{background:var(--aobo-hover) !important;border-color:var(--aobo-accent) !important;}\n  .ts-props .ts-chip.on{background:var(--aobo-accent) !important;border-color:var(--aobo-accent) !important;color:#fff !important;}\n  .ts-count{font-size:.8em;color:var(--aobo-muted);margin-left:auto;white-space:nowrap;}\n\n  \/* Table *\/\n  .ts-table-wrap{overflow-x:auto;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);\n    background:#fff;box-shadow:0 1px 2px rgba(16,24,40,.04);}\n  table.ts-table{border-collapse:collapse;width:100%;min-width:880px;font-size:.88em;}\n  .ts-table thead th{position:sticky;top:0;z-index:2;background:var(--aobo-accent-dark);color:#fff;\n    border-bottom:0;border-right:1px solid rgba(255,255,255,.1);text-align:center;padding:.6em .7em;\n    font-size:.82em;font-weight:600;text-transform:none;letter-spacing:.02em;cursor:pointer;\n    white-space:nowrap;user-select:none;}\n  .ts-table thead th:last-child{border-right:0;}\n  .ts-table thead th .ts-arr{color:#ffd166;font-weight:700;margin-left:3px;}\n  .ts-table tbody td{padding:.55em .7em;border-bottom:1px solid var(--aobo-border);text-align:center;\n    vertical-align:middle;white-space:nowrap;}\n  .ts-table tbody tr:nth-child(even){background:var(--aobo-stripe);}\n  .ts-table tbody tr:hover{background:var(--aobo-hover);}\n  .ts-table tbody tr.ts-group td{background:#e8ecf1;font-weight:700;font-size:.78em;letter-spacing:.05em;\n    text-transform:uppercase;color:#3c4043;padding:.55em .7em;border-bottom:1px solid var(--aobo-border);\n    text-align:left;}\n  .ts-table tbody tr:not(.ts-group).ts-hide{display:none;}\n  td.ts-grade{font-weight:700;font-size:.95em;text-align:left;white-space:nowrap;color:var(--aobo-text);}\n  .ts-meter{display:inline-flex;align-items:center;gap:7px;}\n  .ts-meter i{display:inline-block;width:44px;height:6px;border-radius:3px;background:var(--aobo-fill);overflow:hidden;}\n  .ts-meter i b{display:block;height:100%;border-radius:3px;background:linear-gradient(90deg,#4d94ff,var(--aobo-accent));}\n  .ts-meter span{font-size:.9em;font-weight:600;min-width:14px;}\n  .ts-hr{font-variant-numeric:tabular-nums;font-weight:500;}\n  .ts-num{font-variant-numeric:tabular-nums;}\n  .ts-sup{font-size:9px;color:var(--aobo-accent);vertical-align:super;line-height:0;}\n\n  \/* Footnotes *\/\n  .ts-notes-list{margin:1.2em 0 0;background:#fff;border:1px solid var(--aobo-border);\n    border-left:3px solid var(--aobo-accent);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;\n    padding:1em 1.2em 1em 2.2em;font-size:.82em;color:var(--aobo-muted);line-height:1.7;}\n  .ts-notes-list li{margin-bottom:.3em;}\n  .ts-notes-list sup{color:var(--aobo-accent);font-size:10px;}\n\n  \/* Figure *\/\n  .ts-fig{margin:1.2em 0 0;background:#fff;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);padding:1em;}\n  .ts-fig img{display:block;width:100%;height:auto;border-radius:6px;}\n  .ts-fig figcaption{font-size:.8em;color:var(--aobo-muted);margin-top:.6em;line-height:1.6;}\n  .ts-fig figcaption b{color:var(--aobo-text);}\n\n  \/* Info cards *\/\n  .ts-grid{display:grid;grid-template-columns:repeat(auto-fit,minmax(250px,1fr));gap:14px;margin-top:1.2em;}\n  .ts-grid .ts-card{background:#fff;border:1px solid var(--aobo-border);border-left:3px solid var(--aobo-accent);\n    border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;padding:1em 1.2em;}\n  .ts-grid h2{font-size:1em;margin:0 0 .4em;color:var(--aobo-text);}\n  .ts-grid p{font-size:.82em;color:var(--aobo-muted);margin:0;line-height:1.7;}\n  .ts-grid p b{color:var(--aobo-text);font-weight:600;}\n\n  \/* Disclaimer *\/\n  .ts-disclaimer{margin-top:1.2em;background:#fff;border:1px solid var(--aobo-border);\n    border-left:3px solid var(--aobo-accent);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;\n    padding:1em 1.2em;}\n  .ts-disclaimer h3{margin:0 0 .5em;font-size:.95em;color:var(--aobo-text);display:flex;align-items:center;gap:6px;}\n  .ts-disclaimer h3::before{content:\"\\2139\";font-size:1em;color:var(--aobo-accent);}\n  .ts-disclaimer p{margin:0 0 .5em;max-width:none;color:var(--aobo-muted);line-height:1.7;}\n  .ts-disclaimer p:last-child{margin-bottom:0;}\n\n  \/* Empty \/ source *\/\n  .ts-empty{display:none;text-align:center;color:var(--aobo-muted);padding:2em 1em;font-size:.9em;}\n  .ts-empty.show{display:block;}\n  .ts-source{margin-top:.8em;color:var(--aobo-muted);font-size:.82em;line-height:1.58;}\n\n  @media (max-width:860px){\n    .ts-hero-top,.ts-tool-area{padding:1em;}\n    .ts-controls{flex-direction:column;align-items:stretch;}\n    .ts-search{max-width:none;}\n    .ts-count{margin-left:0;}\n    .ts-hero h1{font-size:1.5rem;}\n  }\n  @media (max-width:520px){\n    .ts-hero-top,.ts-tool-area{padding:.8em;}\n    table.ts-table{font-size:.82em;}\n    .ts-table thead th,.ts-table tbody td{padding:.4em .4em;}\n  }\n  table.ts-table thead th{cursor:default;}\n  table.ts-table td.ts-grade{font-weight:700;}\n  table.ts-table td.ts-type{white-space:normal;text-align:left;font-size:.92em;color:#555;min-width:150px;}\n  table.ts-table td.ts-long{white-space:normal;text-align:left;vertical-align:top;font-size:.92em;color:#444;\n    min-width:260px;line-height:1.55;}\n  table.ts-table td.ts-safe{white-space:normal;text-align:left;vertical-align:top;}\n  table.ts-table tbody tr:hover{background:var(--aobo-hover);}\n  table.ts-table tbody tr.ts-group:hover td{background:#e8ecf1;}\n  .ts-sec{margin:1.8em 0 .5em;font-size:1.02em;color:var(--aobo-text);font-weight:700;}\n  .ts-sec span{display:block;font-size:.8em;font-weight:400;color:var(--aobo-muted);margin-top:.15em;line-height:1.6;}\n  .ts-table-wrap{margin-top:.6em;}\n  .ts-tcap{margin:.5em 0 0;font-size:.78em;color:var(--aobo-muted);line-height:1.6;}\n  .ts-props a{color:var(--aobo-blue) !important;text-decoration:none !important;}\n  .ts-props a:hover{text-decoration:underline !important;}\n  .ts-rel{margin-top:1.2em;background:#fff;border:1px solid var(--aobo-border);\n    border-left:3px solid var(--aobo-blue);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;padding:1em 1.2em;}\n  .ts-rel h3{margin:0 0 .5em;font-size:.95em;color:var(--aobo-text);}\n  .ts-rel p{margin:0;font-size:.85em;line-height:1.9;color:var(--aobo-muted);}\n  .ts-rel p a{font-weight:600;}\n\n  .aobo-ht-ref.ts-props table.ts-table.wraphead thead th{white-space:normal;line-height:1.25;}\n  .aobo-ht-ref.ts-props table.ts-table.wraphead tbody td{white-space:nowrap !important;}\n<\/style>\n\n<style id=\"aobo-dl-css\">\n.aobo-ht-ref.ts-props .ts-dl{display:flex !important;flex-wrap:wrap;align-items:center;gap:1em;\n  background:var(--aobo-stripe) !important;border:1px solid var(--aobo-border) !important;\n  border-radius:var(--aobo-radius) !important;padding:1.1em 1.3em !important;margin:1.5em 0 !important;}\n.aobo-ht-ref.ts-props .ts-dl-txt{flex:1 1 340px;font-size:.95em;color:var(--aobo-text) !important;line-height:1.55;}\n.aobo-ht-ref.ts-props .ts-dl-txt strong{display:block;font-weight:700 !important;margin-bottom:.2em;color:var(--aobo-text) !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn{display:inline-flex !important;align-items:center;gap:.5em;\n  background:var(--aobo-blue) !important;color:#fff !important;border:1px solid var(--aobo-blue) !important;\n  border-radius:var(--aobo-radius-sm) !important;padding:.75em 1.35em !important;font-size:.95em !important;\n  font-weight:600 !important;text-decoration:none !important;white-space:nowrap;box-shadow:none !important;\n  line-height:1.3 !important;text-transform:none !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn:hover,.aobo-ht-ref.ts-props a.ts-dl-btn:focus{background:var(--aobo-blue-dark) !important;\n  border-color:var(--aobo-blue-dark) !important;color:#fff !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn svg{width:1.05em;height:1.05em;fill:none;stroke:currentColor;stroke-width:2;flex:0 0 auto;}\n@media (max-width:640px){.aobo-ht-ref.ts-props a.ts-dl-btn{width:100%;justify-content:center;}}\n<\/style>\n\n<style id=\"aobo-ds\">\n.entry-content[class]{--ds-font-body: Lora,serif;--ds-font-head: Lato,sans-serif;--ds-blue: #0c56d0;--ds-blue-deep: #082d6f;--ds-blue-dark: #073b91;--ds-blue-soft: #eaf2ff;--ds-blue-pale: #f7fbff;--ds-border: #d7e5fb;--ds-border-soft: #e8eef8;--ds-text: #203044;--ds-muted: #617087;--ds-orange: #f59b23;--ds-shadow: 0 18px 45px rgba(12,86,208,0.10);--ds-shadow-sm: 0 12px 32px rgba(12,86,208,0.07);font-family: var(--ds-font-body);line-height: 1.7;-webkit-text-size-adjust: 100%;box-sizing: border-box}.entry-content[class] *,.entry-content[class] *::before,.entry-content[class] *::after{box-sizing: border-box}.entry-content[class] h1{font-family: var(--ds-font-head) !important;font-size: clamp(24px,4vw,min(50px,var(--h1-max,50px))) !important;line-height: 1.08 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 0 0 16px !important}.entry-content[class] h2{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 44px 0 16px !important}.entry-content[class] h3{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.3 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 30px 0 12px !important}.entry-content[class] h4{font-family: var(--ds-font-head) !important;font-size: 19px !important;line-height: 1.35 !important;letter-spacing: 0 !important;font-weight: 700 !important;margin: 24px 0 10px !important}.entry-content[class] p,.entry-content[class] li,.entry-content[class] dd,.entry-content[class] dt{font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important}.entry-content[class] figcaption,.entry-content[class] small,.entry-content[class] .aobo-figure figcaption{font-size: 15px !important;line-height: 1.6 !important}.entry-content[class] table{width: 100%;border-collapse: collapse;background: #ffffff}.entry-content[class] table th,.entry-content[class] table thead th,.entry-content[class] table thead td{background: var(--ds-blue-soft) !important;color: var(--ds-blue-deep) !important;font-family: var(--ds-font-head) !important;font-size: 15px !important;font-weight: 700 !important;line-height: 1.45 !important;text-align: center !important;text-transform: none !important;letter-spacing: 0 !important;padding: 14px 16px !important;border: 0 !important;border-bottom: 1px solid var(--ds-border) !important;vertical-align: top !important;position: static !important}.entry-content[class] table td{font-family: var(--ds-font-body) !important;font-size: 15px !important;line-height: 1.55 !important;padding: 14px 16px !important;border: 0;border-bottom: 1px solid var(--ds-border-soft) !important;vertical-align: top !important;white-space: normal !important;text-align: center !important}.entry-content[class] table tbody tr:last-child td{border-bottom: 0 !important}.entry-content[class] table th.ds-text,.entry-content[class] table td.ds-text{text-align: left !important}.entry-content[class] table tbody tr:nth-child(even){background: #fafcff !important}.entry-content[class] table tbody tr:hover{background: #f2f7ff !important}.entry-content[class] table tbody td:first-child{color: var(--ds-blue-deep);font-weight: 700}.entry-content[class] .aobo-table-wrap,.entry-content[class] .ts-table-wrap{overflow-x: auto;margin: 22px 0 28px;border: 1px solid var(--ds-border);border-radius: 18px;box-shadow: var(--ds-shadow-sm);background: #ffffff}.entry-content[class] h1,.entry-content[class] h2,.entry-content[class] h3,.entry-content[class] h4{color: var(--ds-blue-deep)}.entry-content[class] p,.entry-content[class] li{color: var(--ds-text)}.entry-content[class] a{color: var(--ds-blue);font-weight: 700;text-decoration: none}.entry-content[class] a:hover,.entry-content[class] a:focus{color: var(--ds-orange)}.entry-content[class] .aobo-final-cta h1,.entry-content[class] .aobo-final-cta h2,.entry-content[class] .aobo-final-cta h3,.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-cta h1,.entry-content[class] .aobo-cta h2,.entry-content[class] .aobo-cta h3,.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-cta-buttons,.entry-content[class] .aobo-cta-buttons *,.entry-content[class] .aobo-esr .stat-band h2,.entry-content[class] .aobo-esr .stat-band h3,.entry-content[class] .aobo-esr .stat-band p,.entry-content[class] .aobo-esr .closing h2,.entry-content[class] .aobo-esr .closing h3,.entry-content[class] .aobo-esr .closing p,.entry-content[class] .footcta h2,.entry-content[class] .footcta h3,.entry-content[class] .footcta p,.entry-content[class] .bg-dark h2,.entry-content[class] .bg-dark h3,.entry-content[class] .bg-dark p,.entry-content[class] .ht-header h2,.entry-content[class] .ht-header h3,.entry-content[class] .ts-cta h2,.entry-content[class] .ts-cta h3,.entry-content[class] .aobo-sup .stats h2,.entry-content[class] .aobo-sup .stats h3,.entry-content[class] .aobo-sup .stats p,.entry-content[class] .aobo-sup .cta h2,.entry-content[class] .aobo-sup .cta h3,.entry-content[class] .aobo-sup .cta p{color: inherit}.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-sup .cta p{color: rgba(255,255,255,0.92)}.entry-content[class] .has-ast-global-color-0-background-color,.entry-content[class] .has-ast-global-color-0-background-color *,.entry-content[class] .contact-container,.entry-content[class] .contact-container *{color: #ffffff !important}.entry-content[class] .has-ast-global-color-0-background-color .label-text,.entry-content[class] .has-ast-global-color-0-background-color .label-text *,.entry-content[class] .contact-container .label-text{color: rgba(255,255,255,0.72) !important}.entry-content[class] .aobo-cta h1,.entry-content[class] .aobo-cta h2,.entry-content[class] .aobo-cta h3,.entry-content[class] .aobo-cta h4,.entry-content[class] .cta h1,.entry-content[class] .cta h2,.entry-content[class] .cta h3,.entry-content[class] .cta h4,.entry-content[class] .aobo-final-cta h1,.entry-content[class] .aobo-final-cta h2,.entry-content[class] .aobo-final-cta h3,.entry-content[class] .aobo-final-cta h4{color: #ffffff !important}.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-cta li,.entry-content[class] .cta p,.entry-content[class] .cta li,.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-final-cta li{color: rgba(255,255,255,0.93) !important}.entry-content[class] .aobo-cta p a,.entry-content[class] .aobo-cta li a,.entry-content[class] .cta p a,.entry-content[class] .cta li a,.entry-content[class] .aobo-final-cta p a,.entry-content[class] .aobo-final-cta li a{color: #ffffff !important;text-decoration: underline}.entry-content[class] .aobo-btn-inquiry{color: #ffffff !important}.entry-content[class] .aobo-cta .aobo-btn-inquiry,.entry-content[class] .aobo-final-cta .aobo-btn-inquiry{color: var(--ds-blue) !important}.entry-content[class] .aobo-wrap,.entry-content[class] .aobo-article{max-width: 1180px;margin: 0 auto;padding: 0}.entry-content[class] img{max-width: 100%;height: auto}.entry-content[class] figure{margin: 26px auto 34px;max-width: 860px}.entry-content[class] figure img{display: block;width: 100%;border: 1px solid var(--ds-border);border-radius: 18px;box-shadow: var(--ds-shadow-sm);background: #ffffff}.entry-content[class] .aobo-hero{background: linear-gradient(135deg,#ffffff 0%,#f7fbff 56%,#eaf2ff 100%);border: 1px solid var(--ds-border);border-radius: 28px;padding: 42px 38px;margin-bottom: 24px;box-shadow: var(--ds-shadow);overflow: hidden;position: relative}.entry-content[class] .aobo-hero::after{content: \"\";position: absolute;right: -90px;top: -90px;width: 260px;height: 260px;border-radius: 50%;background: rgba(12,86,208,0.08)}.entry-content[class] .aobo-hero h1,.entry-content[class] .aobo-hero p{position: relative;z-index: 2}.entry-content[class] .aobo-note-box{margin: 34px 0;padding: 22px 24px;border: 1px solid var(--ds-border);border-left: 5px solid var(--ds-orange);border-radius: 16px;background: #fbfdff}.entry-content[class] .aobo-note-box p{margin: 0 0 14px;color: var(--ds-muted) !important;font-style: italic}.entry-content[class] .aobo-note-box p:last-child{margin-bottom: 0}.entry-content[class] .aobo-btn{display: inline-flex;align-items: center;justify-content: center;min-height: 42px;padding: 10px 16px;border-radius: 999px;text-align: center;text-decoration: none;font-family: var(--ds-font-head) !important;font-weight: 700;font-size: 14px !important;line-height: 1.2;transition: all 0.2s ease;cursor: pointer;white-space: nowrap}.entry-content[class] .aobo-btn-primary{background: var(--ds-blue);border: 1px solid var(--ds-blue);color: #ffffff !important}.entry-content[class] .aobo-btn-secondary{background: #ffffff;border: 1px solid var(--ds-border);color: var(--ds-blue) !important}.entry-content[class] .aobo-btn:hover{transform: translateY(-1px)}.entry-content[class] .aobo-supply-actions{display: flex;flex-wrap: wrap;gap: 12px;margin-top: 18px}.entry-content[class] .aobo-supply-actions .aobo-btn{min-width: 190px}.entry-content[class] .aobo-final-cta{margin-top: 34px;padding: 34px;border-radius: 28px;background: linear-gradient(135deg,#073b91 0%,#0c56d0 100%);box-shadow: 0 18px 45px rgba(12,86,208,0.20);display: flex;align-items: center;justify-content: space-between;gap: 20px;flex-wrap: wrap}.entry-content[class] .aobo-final-cta h2{margin: 0 0 12px !important;font-size: 26px !important;color: #ffffff !important}.entry-content[class] .aobo-final-cta p{margin: 0}.entry-content[class] .aobo-final-cta .aobo-btn-primary{background: #ffffff;border-color: #ffffff;color: var(--ds-blue) !important}.entry-content[class] .aobo-final-cta .aobo-btn-secondary{background: transparent;border-color: rgba(255,255,255,0.75);color: #ffffff !important}.entry-content[class] .ts-hero{background: transparent !important;border: 0 !important;border-radius: 0 !important;box-shadow: none !important}.entry-content[class] .ts-hero-top{background: linear-gradient(135deg,#ffffff 0%,#f7fbff 56%,#eaf2ff 100%) !important;border: 1px solid var(--ds-border) !important;border-radius: 28px !important;padding: 42px 38px !important;margin: 0 0 24px !important;box-shadow: var(--ds-shadow) !important;position: relative;overflow: hidden;text-align: left !important}.entry-content[class] .ts-hero-top h1,.entry-content[class] .ts-hero-top p,.entry-content[class] .ts-hero h1{text-align: left !important}.entry-content[class] .ts-hero-top p{max-width: none !important;margin: 0 0 12px !important}.entry-content[class] .ts-tool-area{padding: 0 !important}.entry-content[class] .ts-sec{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 44px 0 16px !important}.entry-content[class] .ts-sec > span{display: block !important;font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important;font-weight: 400 !important;color: var(--ds-text) !important;margin: 0 0 16px !important}.entry-content[class] .ts-kicker{display: inline-flex !important;align-items: center;gap: 7px;margin: 0 0 14px !important;padding: 6px 14px !important;border: 1px solid var(--ds-border) !important;border-radius: 999px !important;background: #ffffff !important;color: var(--ds-blue) !important;font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important;letter-spacing: 0 !important;text-transform: none !important}.entry-content[class] .ts-p,.entry-content[class] .card-desc,.entry-content[class] .aobo-strip-intro,.entry-content[class] .schema-faq-answer{font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important;font-weight: 400 !important}.entry-content[class] .lead,.entry-content[class] .fund-lead{font-family: var(--ds-font-body) !important;font-size: 19px !important;line-height: 1.65 !important;font-weight: 400 !important}.entry-content[class] .ts-h2{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 44px 0 16px !important}.entry-content[class] .ts-h3{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.3 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 30px 0 12px !important}.entry-content[class] .card-grade{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.25 !important;font-weight: 700 !important}.entry-content[class] .schema-faq-question{font-family: var(--ds-font-head) !important;font-size: 19px !important;line-height: 1.4 !important;font-weight: 700 !important;color: var(--ds-blue-deep) !important}.entry-content[class] .ts-source,.entry-content[class] .ts-hint,.entry-content[class] .ts-placeholder,.entry-content[class] .ht-spec-label,.entry-content[class] .ht-spec-value,.entry-content[class] .ht-step-indicator,.entry-content[class] .ht-badge,.entry-content[class] .idx,.entry-content[class] .xlink,.entry-content[class] .cat-note,.entry-content[class] .aobo-card-note,.entry-content[class] .card-desig,.entry-content[class] .k,.entry-content[class] .v,.entry-content[class] .note,.entry-content[class] .aobo-note{font-family: var(--ds-font-head) !important;font-size: 15px !important;line-height: 1.6 !important;font-weight: 400 !important}.entry-content[class] .ht-spec-label,.entry-content[class] .idx,.entry-content[class] .k{font-weight: 700 !important}.entry-content[class] .aobo-note,.entry-content[class] .note{font-family: var(--ds-font-body) !important;color: var(--ds-muted) !important}.entry-content[class] .chip{font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important}.entry-content[class] .kicker,.entry-content[class] .eyebrow,.entry-content[class] .aobo-eyebrow{display: inline-flex !important;align-items: center;gap: 7px;margin: 0 0 14px !important;padding: 6px 14px !important;border: 1px solid var(--ds-border) !important;border-radius: 999px !important;background: #ffffff !important;color: var(--ds-blue) !important;font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important;letter-spacing: 0 !important;text-transform: none !important}@media (max-width: 760px){.entry-content[class] h1{font-size: clamp(22px,6.4vw,min(34px,var(--h1-max,34px))) !important}.entry-content[class] h2{font-size: 25px !important}.entry-content[class] h3{font-size: 20px !important}.entry-content[class] h4{font-size: 17px !important}.entry-content[class] p,.entry-content[class] li{font-size: 16px !important}.entry-content[class] table th,.entry-content[class] table td{font-size: 14px !important;padding: 11px 12px !important}.entry-content[class] .aobo-hero{padding: 30px 22px}.entry-content[class] .aobo-final-cta{padding: 26px 22px}.entry-content[class] .aobo-final-cta .aobo-btn{width: 100%}}\n<\/style>\n<section class=\"aobo-ht-ref ts-props\">\n<div class=\"aobo-wrap\">\n\n<div class=\"ts-hero\">\n<div class=\"ts-hero-top\">\n<div class=\"ts-kicker\"><span><\/span>Tool Steel | Die Casting | Thermal Fatigue<\/div>\n<h1 style=\"--h1-max:38px\">Thermal Fatigue Cracking in Die Casting Dies<\/h1>\n<p>Thermal fatigue cracking is the most common way an aluminium die casting die ends its working life. It begins as a fine crack network on the hottest corners and grows until the die has to be pulled for repair. This page sets out the four failure modes a die faces, how the thermal stress that drives the crack is built and released in every cycle, and the temperature and cracking data measured in a controlled immersion test on premium grade H13.<\/p>\n<\/div>\n<\/div>\n\n<div class=\"ts-tool-area\">\n\n<h2 class=\"ts-h2\">The four ways a die fails<\/h2>\n<p class=\"ts-p\">The source lists four main failure modes for an aluminium die casting die. Physical erosion, also called washing, where a fast flow of melt scours the surface and gets worse when hard particles are carried in the melt. Chemical attack, or corrosion, where the melt dissolves the steel and forms interphase layers when the relative motion between the steel and the melt is small. Gross cracking, a cleavage fracture through the die that can be complete and sudden, and that starts from a combination of thermal and mechanical stress. And thermal fatigue cracking, also called heat checking, which is the slow crack network that this page is about.<\/p>\n\n<h2 class=\"ts-h2\">How the stress is built and released in each cycle<\/h2>\n<p class=\"ts-p\">Thermal stress appears when the free expansion or contraction of the steel is restrained. In a die the restraint is mostly internal, because a temperature gradient across the section means the hot surface wants to expand more than the cooler mass behind it. For a bar with fixed ends the stress from a temperature change is the expansion coefficient multiplied by the elastic modulus and by the change in temperature. In a biaxial condition the same product is divided by one minus the Poisson ratio. Both the expansion coefficient and the modulus change with temperature, so the full stress never develops, but the gradient is what drives it.<\/p>\n<p class=\"ts-p\">When the melt is injected, the surface is put in compression against the cooler interior. When the part is ejected and the lubricant is sprayed, the surface cools faster than the interior, the compression is relieved, and tension appears. Once the local deformation turns plastic, cycle after cycle, a crack starts. The crack then grows along a plane at right angles to the largest tensile stress, through the stages of initiation at the surface, linking of small cracks at the surface, growth of the crack network into the depth, and finally the growth of the largest crack until the die fails.<\/p>\n\n<h2 class=\"ts-h2\">Longer contact with the melt raises the temperature and the damage<\/h2>\n<p class=\"ts-p\">The source test dunked premium grade H13 specimens into molten aluminium held at 1350 F for 5, 7, 9 and 12 seconds, with the specimen withdrawn for 24 seconds between immersions and water run through the internal cooling line throughout. Immersion time was the only variable. Cracks were measured after 5,000, 10,000 and 15,000 cycles. The table gives the results at 15,000 cycles. The peak temperature rises by 221 F from the shortest to the longest immersion, and the total crack area rises from 1.97 to 167.72, about eighty five times larger.<\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\">\n<thead>\n<tr>\n<th style=\"width:36%\">Item<\/th><th>5 sec<\/th><th>7 sec<\/th><th>9 sec<\/th><th>12 sec<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr><td class=\"ts-grade\">Maximum temperature, F<\/td><td class=\"ts-safe\">926<\/td><td class=\"ts-safe\">991<\/td><td class=\"ts-safe\">1087<\/td><td class=\"ts-safe\">1147<\/td><\/tr>\n<tr><td class=\"ts-grade\">Minimum temperature, F<\/td><td class=\"ts-safe\">322<\/td><td class=\"ts-safe\">346<\/td><td class=\"ts-safe\">399<\/td><td class=\"ts-safe\">460<\/td><\/tr>\n<tr><td class=\"ts-grade\">Total crack area, x 10<sup>6<\/sup> &micro;m<sup>2<\/sup>, after 15,000 cycles<\/td><td class=\"ts-safe\">1.97<\/td><td class=\"ts-safe\">5.9<\/td><td class=\"ts-safe\">108.56<\/td><td class=\"ts-safe\">167.72<\/td><\/tr>\n<tr><td class=\"ts-grade\">Average maximum crack length, x 100 &micro;m, after 15,000 cycles<\/td><td class=\"ts-safe\">2.25<\/td><td class=\"ts-safe\">3<\/td><td class=\"ts-safe\">12.5<\/td><td class=\"ts-safe\">15.25<\/td><\/tr>\n<tr><td class=\"ts-grade\">Hardness at the average maximum crack length, HRC<\/td><td class=\"ts-safe\">36.9<\/td><td class=\"ts-safe\">33.8<\/td><td class=\"ts-safe\">31.6<\/td><td class=\"ts-safe\">29.2<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>The effect of immersion time on the temperature at the corner of a premium H13 specimen and on the cracking measured after 15,000 cycles. Immersion time is the only variable, and the cooling line was 1.5 in in every case.<\/em><\/p>\n\n<h2 class=\"ts-h2\">Hardness falls from the corner inward<\/h2>\n<p class=\"ts-p\">The cracking follows the softening, and the softening follows the temperature. The table below gives the hardness measured from the corner inward at 15,000 cycles for the same four immersion times. The 5 and 7 second specimens hold most of their hardness to within 0.1 in of the corner. The 9 and 12 second specimens lose twenty or more points at the corner and are still soft at 0.2 in into the steel.<\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\">\n<thead>\n<tr>\n<th style=\"width:36%\">Distance from the corner, in<\/th><th>5 sec<\/th><th>7 sec<\/th><th>9 sec<\/th><th>12 sec<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr><td class=\"ts-grade\">0.01<\/td><td class=\"ts-safe\">36.9<\/td><td class=\"ts-safe\">33.8<\/td><td class=\"ts-safe\">24.5<\/td><td class=\"ts-safe\">24.3<\/td><\/tr>\n<tr><td class=\"ts-grade\">0.02<\/td><td class=\"ts-safe\">39.4<\/td><td class=\"ts-safe\">36.5<\/td><td class=\"ts-safe\">27.4<\/td><td class=\"ts-safe\">25.1<\/td><\/tr>\n<tr><td class=\"ts-grade\">0.04<\/td><td class=\"ts-safe\">42.4<\/td><td class=\"ts-safe\">39.1<\/td><td class=\"ts-safe\">31.2<\/td><td class=\"ts-safe\">27.7<\/td><\/tr>\n<tr><td class=\"ts-grade\">0.06<\/td><td class=\"ts-safe\">43.3<\/td><td class=\"ts-safe\">42.4<\/td><td class=\"ts-safe\">32.3<\/td><td class=\"ts-safe\">29.2<\/td><\/tr>\n<tr><td class=\"ts-grade\">0.08<\/td><td class=\"ts-safe\">44.1<\/td><td class=\"ts-safe\">44.2<\/td><td class=\"ts-safe\">34.5<\/td><td class=\"ts-safe\">29.2<\/td><\/tr>\n<tr><td class=\"ts-grade\">0.1<\/td><td class=\"ts-safe\">44.3<\/td><td class=\"ts-safe\">44.3<\/td><td class=\"ts-safe\">36.2<\/td><td class=\"ts-safe\">30<\/td><\/tr>\n<tr><td class=\"ts-grade\">0.2<\/td><td class=\"ts-safe\">44.4<\/td><td class=\"ts-safe\">44.5<\/td><td class=\"ts-safe\">40.9<\/td><td class=\"ts-safe\">34.1<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Hardness in HRC measured from the corner inward on the four specimens after 15,000 cycles. The greater the immersion time, the deeper and softer the softened band.<\/em><\/p>\n\n<h2 class=\"ts-h2\">Estimating the stress at the corner<\/h2>\n<p class=\"ts-p\">With the expansion coefficient and modulus of H13, 6.9 micro inch per inch per F and 30,500 ksi, the axial stress range at the corner of the 12 second, 1.5 in cooling line specimen works out at about 145 ksi, using the temperature range measured at the corner. That figure agrees closely with the computer model the source ran for the same specimen. During immersion the corner is in high compression, and because the yield strength of the steel falls at temperature, that compression can go plastic. What is left behind is a residual tension, well below the yield strength but high enough to start a crack at any <a href=\"https:\/\/aobosteel.com\/tool-and-die-design-faults\/\">stress raiser<\/a> such as a machining mark or a corrosion pit.<\/p>\n<div class=\"ts-dl\"><div class=\"ts-dl-txt\"><strong>Thermal fatigue cracking in die casting dies, printable PDF<\/strong> The temperature and cracking data for four immersion times, the hardness profiles behind them, and the stress calculation for the corner, in one reference sheet with our contact details.<\/div> <a class=\"ts-dl-btn\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Thermal-Fatigue-Cracking-Die-Casting-Dies.pdf\" download> <svg viewBox=\"0 0 24 24\" aria-hidden=\"true\"><path d=\"M12 3v12m0 0 4.5-4.5M12 15l-4.5-4.5M4 20h16\"\/><\/svg> Download PDF <\/a><\/div>\n\n<h2 class=\"ts-h2\">What this means on the job<\/h2>\n<p class=\"ts-p\">The steel in these tests is <a href=\"https:\/\/aobosteel.com\/nadca-229-die-steel-acceptance-criteria\/\">premium grade H13<\/a>, the chromium hot work steel covered on the <a href=\"https:\/\/aobosteel.com\/h13-tool-steel\/\">H13 tool steel page<\/a> and held as die stock on the <a href=\"https:\/\/aobosteel.com\/1-2344-esr-h13-aluminum-extrusion-distributors\/\">1.2344 ESR H13 supply page<\/a>. The general resistance of the hot work grades is compared on the <a href=\"https:\/\/aobosteel.com\/thermal-fatigue-resistant-tool-steels\/\">thermal fatigue resistant tool steels page<\/a>, and why H13 is the default for a die is set out on the <a href=\"https:\/\/aobosteel.com\/blog\/why-h13-steel-used-in-die-casting\/\">why H13 steel is used in die casting page<\/a>. The cooling design that holds the peak temperature down is on the <a href=\"https:\/\/aobosteel.com\/die-casting-die-cooling-line-design\/\">die cooling line design page<\/a>, and the softening behind the crack on the <a href=\"https:\/\/aobosteel.com\/h13-die-softening-in-service\/\">H13 die softening page<\/a>. The other failure modes are on the <a href=\"https:\/\/aobosteel.com\/die-wear-and-failure-mechanisms\/\">die wear and failure page<\/a> and the <a href=\"https:\/\/aobosteel.com\/tool-and-die-failure-analysis\/\">tool and die failure analysis page<\/a>. The loss of hardness at temperature is on the <a href=\"https:\/\/aobosteel.com\/hot-work-tool-steel-softening-resistance\/\">hot work softening resistance page<\/a>, the properties that set the gradient on the <a href=\"https:\/\/aobosteel.com\/tool-steel-thermal-conductivity\/\">thermal conductivity page<\/a>, and the way a grade is chosen for a press on the <a href=\"https:\/\/aobosteel.com\/selection-of-tool-steel-for-high-pressure-die-casting-dies\/\">high pressure die casting selection page<\/a>.<\/p>\n\n<div class=\"ts-disclaimer\">\n<h3>Before you use this as a die design specification<\/h3>\n<p>This page is a reference summary of a published study and it is not an Aobo Steel specification. The temperature, cracking and hardness values are reproduced from the source, which tested one grade, one specimen shape and one set of casting conditions. The cracking a production die develops also depends on the die design, the alloy, the cycle and the shot weight. Final die design is confirmed on the job.<\/p>\n<\/div>\n\n<p class=\"ts-source\">Source, Effect of Design Factors on Thermal Fatigue Cracking of Die Casting Dies, D. Schwam, J. F. Wallace and S. Birceanu, Case Western Reserve University, final technical report to the U.S. Department of Energy, Award No. DE-FC07-00ID138486, October 2004.<\/p>\n\n<\/div><\/div><\/section>\n\n","protected":false},"excerpt":{"rendered":"<p>Tool Steel | Die Casting | Thermal Fatigue Thermal Fatigue Cracking in Die Casting Dies Thermal fatigue cracking is the most common way an aluminium die casting die ends its working life. It begins as a fine crack network on the hottest corners and grows until the die has to be pulled for repair. This [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-21450","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.6 (Yoast SEO v28.6) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Thermal Fatigue Cracking in Die Casting Dies | Aobo Steel<\/title>\n<meta name=\"description\" content=\"How thermal fatigue cracking starts in aluminium die casting dies, with temperature, cracking and hardness data for four melt contact times in premium H13.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/thermal-fatigue-cracking-in-die-casting-dies\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Thermal Fatigue Cracking in Die Casting Dies\" \/>\n<meta property=\"og:description\" content=\"How thermal fatigue cracking starts in aluminium die casting dies, with temperature, cracking and hardness data for four melt contact times in premium H13.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/thermal-fatigue-cracking-in-die-casting-dies\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-11T03:02:02+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"6 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/thermal-fatigue-cracking-in-die-casting-dies\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/thermal-fatigue-cracking-in-die-casting-dies\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Thermal Fatigue Cracking in Die Casting Dies\",\"datePublished\":\"2026-10-09T04:36:25+00:00\",\"dateModified\":\"2026-10-11T03:02:02+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/thermal-fatigue-cracking-in-die-casting-dies\\\/\"},\"wordCount\":1157,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/thermal-fatigue-cracking-in-die-casting-dies\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/thermal-fatigue-cracking-in-die-casting-dies\\\/\",\"name\":\"Thermal Fatigue Cracking in Die Casting Dies | Aobo Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-09T04:36:25+00:00\",\"dateModified\":\"2026-10-11T03:02:02+00:00\",\"description\":\"How thermal fatigue cracking starts in aluminium die casting dies, with temperature, cracking and hardness data for four melt contact times in premium H13.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/thermal-fatigue-cracking-in-die-casting-dies\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/thermal-fatigue-cracking-in-die-casting-dies\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/thermal-fatigue-cracking-in-die-casting-dies\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Thermal Fatigue Cracking in Die Casting Dies\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Thermal Fatigue Cracking in Die Casting Dies | Aobo Steel","description":"How thermal fatigue cracking starts in aluminium die casting dies, with temperature, cracking and hardness data for four melt contact times in premium H13.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/thermal-fatigue-cracking-in-die-casting-dies\/","og_locale":"pt_BR","og_type":"article","og_title":"Thermal Fatigue Cracking in Die Casting Dies","og_description":"How thermal fatigue cracking starts in aluminium die casting dies, with temperature, cracking and hardness data for four melt contact times in premium H13.","og_url":"https:\/\/aobosteel.com\/pt\/thermal-fatigue-cracking-in-die-casting-dies\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-11T03:02:02+00:00","twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"6 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/thermal-fatigue-cracking-in-die-casting-dies\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/thermal-fatigue-cracking-in-die-casting-dies\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Thermal Fatigue Cracking in Die Casting Dies","datePublished":"2026-10-09T04:36:25+00:00","dateModified":"2026-10-11T03:02:02+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/thermal-fatigue-cracking-in-die-casting-dies\/"},"wordCount":1157,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/thermal-fatigue-cracking-in-die-casting-dies\/","url":"https:\/\/aobosteel.com\/thermal-fatigue-cracking-in-die-casting-dies\/","name":"Thermal Fatigue Cracking in Die Casting Dies | Aobo Steel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-09T04:36:25+00:00","dateModified":"2026-10-11T03:02:02+00:00","description":"How thermal fatigue cracking starts in aluminium die casting dies, with temperature, cracking and hardness data for four melt contact times in premium H13.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/thermal-fatigue-cracking-in-die-casting-dies\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/thermal-fatigue-cracking-in-die-casting-dies\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/thermal-fatigue-cracking-in-die-casting-dies\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Thermal Fatigue Cracking in Die Casting Dies"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Tool Steel | Die Casting | Thermal Fatigue Thermal Fatigue Cracking in Die Casting Dies Thermal fatigue cracking is the most common way an aluminium die casting die ends its working life. It begins as a fine crack network on the hottest corners and grows until the die has to be pulled for repair. This&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Tool Steel | Die Casting | Thermal Fatigue Thermal Fatigue Cracking in Die Casting Dies Thermal fatigue cracking is the most common way an aluminium die casting die ends its working life. It begins as a fine crack network on the hottest corners and grows until the die has to be pulled for repair. This&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21450","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=21450"}],"version-history":[{"count":3,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21450\/revisions"}],"predecessor-version":[{"id":21795,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21450\/revisions\/21795"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=21450"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}