{"id":21355,"date":"2026-10-08T18:49:47","date_gmt":"2026-10-08T10:49:47","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=21355"},"modified":"2026-10-19T22:51:26","modified_gmt":"2026-10-19T14:51:26","slug":"galling-of-stainless-tool-steels","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/galling-of-stainless-tool-steels\/","title":{"rendered":"Engripamento de A\u00e7os Inoxid\u00e1veis e Quanto Esfor\u00e7o \u00c9 Necess\u00e1rio"},"content":{"rendered":"<h1 id=\"h-galling-of-stainless-steels-and-how-much-stress-it-takes\" class=\"wp-block-heading\">Engripamento de A\u00e7os Inoxid\u00e1veis e Quanto Esfor\u00e7o \u00c9 Necess\u00e1rio<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">O engripamento \u00e9 a soldagem a frio de pontos microsc\u00f3picos altos entre duas superf\u00edcies deslizantes, e \u00e9 por isso que uma pe\u00e7a de a\u00e7o inoxid\u00e1vel que se movimentava livremente na oficina trava na m\u00e1quina. Todas as cinco fam\u00edlias de a\u00e7o inoxid\u00e1vel s\u00e3o suscet\u00edveis, incluindo os graus martens\u00edticos que uma ferramentaria compra como 420 e 440C. Tamb\u00e9m \u00e9 medido. O ensaio de bot\u00e3o sobre bloco fornece uma tens\u00e3o limite de engripamento para cada grau e condi\u00e7\u00e3o, e a tabela publicada abrange quatro fam\u00edlias e dezesseis designa\u00e7\u00f5es de liga, o suficiente para responder qual inoxid\u00e1vel combinar com o qu\u00ea.<\/p>\n\n\n\n<h2 id=\"h-the-threshold-galling-stress-grade-by-grade\" class=\"wp-block-heading\">A tens\u00e3o limite de engripamento, grau por grau<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">No ensaio de bot\u00e3o sobre bloco, um bot\u00e3o carregado \u00e9 rotacionado contra um bloco do mesmo material at\u00e9 a superf\u00edcie rasgar; a tens\u00e3o de contato nesse ponto \u00e9 a tens\u00e3o limite de engripamento. Um n\u00famero mais alto \u00e9 melhor. As entradas marcadas como n\u00e3o engripantes percorreram toda a faixa do ensaio sem rasgar, portanto compartilham um \u00fanico valor, e as duas colunas de unidades reproduzem a impress\u00e3o da fonte. A dureza \u00e9 dada como a fonte a fornece, em Rockwell B ou Rockwell C.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Grau<\/th><th class=\"has-text-align-left\" data-align=\"left\">Condi\u00e7\u00e3o<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza<\/th><th class=\"has-text-align-left\" data-align=\"left\">MPa<\/th><th class=\"has-text-align-left\" data-align=\"left\">ksi<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\">Austen\u00edtico<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S20161<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">104 (a)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (a)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S21800<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">92 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">104 (a)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (a)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S28200<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">96 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">166<\/td><td class=\"has-text-align-left\" data-align=\"left\">24<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S28200<\/td><td class=\"has-text-align-left\" data-align=\"left\">Trefilado a frio<\/td><td class=\"has-text-align-left\" data-align=\"left\">35 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S20910<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">97 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S20900<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">96 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">48<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S24100<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">23 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">97<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S30430<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">74 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">86 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">Trefilado a frio<\/td><td class=\"has-text-align-left\" data-align=\"left\">27 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">17<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">82 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">48<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">Trefilado a frio<\/td><td class=\"has-text-align-left\" data-align=\"left\">27 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 303<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">85 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">138<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 201<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">104<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">N08020<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">87 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\">Martens\u00edtico<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S42010<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 204 \u00b0C (400 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">50 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">104 (a)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (a)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S42010<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 260 \u00b0C (500 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">47 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 410<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">87 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 410<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 260 \u00b0C (500 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">43 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">21<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 416<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">21<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 416<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 316 \u00b0C (600 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">37 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">62<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 416<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 538 \u00b0C (1000 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">32 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">42<\/td><td class=\"has-text-align-left\" data-align=\"left\">6<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 420<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 204 \u00b0C (400 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">51 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">18<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 420<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 260 \u00b0C (500 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">49 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 440C<\/td><td class=\"has-text-align-left\" data-align=\"left\">Revenido a 260 \u00b0C (500 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">55 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">125<\/td><td class=\"has-text-align-left\" data-align=\"left\">18<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\">Endurec\u00edvel por precipita\u00e7\u00e3o<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45500<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envelhecido a 510 \u00b0C (950 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">48 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">90<\/td><td class=\"has-text-align-left\" data-align=\"left\">13<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45500<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envelhecido a 566 \u00b0C (1050 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">43 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">59<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45500<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envelhecido a 621 \u00b0C (1150 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">36 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">28<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45000<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">29 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">69<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45000<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envelhecido a 480 \u00b0C (895 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">43 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">55<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45000<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envelhecido a 566 \u00b0C (1050 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">17<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45000<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envelhecido a 621 \u00b0C (1150 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">33 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S17400<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envelhecido a 480 \u00b0C (895 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">45 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">69<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S17400<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envelhecido a 621 \u00b0C (1150 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">34 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S13800<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envelhecido a 538 \u00b0C (1000 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">46 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">21<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S66286<\/td><td class=\"has-text-align-left\" data-align=\"left\">Envelhecido a 718 \u00b0C (1325 \u00b0F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"5\">Ferr\u00edtico e duplex<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S18200<\/td><td class=\"has-text-align-left\" data-align=\"left\">Trefilado a frio<\/td><td class=\"has-text-align-left\" data-align=\"left\">98 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">35<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 430F<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">92 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 430<\/td><td class=\"has-text-align-left\" data-align=\"left\">Trefilado a frio<\/td><td class=\"has-text-align-left\" data-align=\"left\">98 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 329<\/td><td class=\"has-text-align-left\" data-align=\"left\">Recozido<\/td><td class=\"has-text-align-left\" data-align=\"left\">25 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Tens\u00e3o limite de engripamento de a\u00e7os inoxid\u00e1veis autoconjugados no ensaio de bot\u00e3o sobre bloco, ASTM G98, acabamento retificado sem lubrifica\u00e7\u00e3o, reproduzido do ASM Handbook, Volume 18. As entradas marcadas com (a) n\u00e3o engriparam dentro da faixa do ensaio. Os valores s\u00e3o impressos como constam na fonte.<\/em><\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>Engripamento de a\u00e7os inoxid\u00e1veis, PDF para impress\u00e3o<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A tens\u00e3o limite de engripamento para cada fam\u00edlia de inoxid\u00e1vel, o ranking de materiais para desgaste adesivo, o volume perdido por ligas comuns e o efeito da temperatura, em um \u00fanico PDF com nossos dados de contato.<\/p>\n\n\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Galling-Of-Stainless-Steels.pdf\">Baixar PDF<\/a><\/div>\n<\/div>\n<\/div>\n\n\n\n<h2 id=\"h-what-the-ranking-says\" class=\"wp-block-heading\">O que o ranking diz<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Entre os graus austen\u00edticos, as ligas cromo-mangan\u00eas-nitrog\u00eanio superam as ligas cromo-n\u00edquel de dureza semelhante. S28200, S20161 e S21800 apresentam os limites mais altos da fam\u00edlia, enquanto N08020, a liga rica em n\u00edquel, apresenta o mais baixo, com 14 MPa. A fonte atribui isso a dois efeitos de liga. O n\u00edquel prejudica a resist\u00eancia ao engripamento, enquanto o sil\u00edcio ajuda, o que explica ambas as extremidades da tabela. O tipo 303, o grau de usinagem livre, situa-se alto, com 138 MPa, devido \u00e0 sua qu\u00edmica e superf\u00edcie usinada, e lembra que um grau escolhido por uma propriedade traz outras propriedades consigo.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Endurecer um grau austen\u00edtico por trefila\u00e7\u00e3o a frio piora sua resist\u00eancia ao engripamento, n\u00e3o melhora. O Tipo 304 cai de 55 MPa recozido a 86 HRB para 17 MPa trefilado a frio a 27 HRC, e o S28200 cai de 166 MPa para 62 MPa na mesma mudan\u00e7a. Esta \u00e9 a linha mais contraintuitiva da tabela, e decorre do mecanismo. A resist\u00eancia ao engripamento nessas ligas vem da capacidade de endurecer por deforma\u00e7\u00e3o exatamente no contato, e um grau que j\u00e1 foi trabalhado a frio gastou essa capacidade antes de a pe\u00e7a entrar em servi\u00e7o.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Entre os graus martens\u00edticos, uma dureza de trabalho mais alta n\u00e3o produz por si s\u00f3 um limite mais alto, e as duas condi\u00e7\u00f5es do Tipo 420 mostram isso claramente. Revenido a 204 C at\u00e9 51 HRC, retorna 25 MPa; revenido a 260 C at\u00e9 49 HRC, retorna 55 MPa, portanto a condi\u00e7\u00e3o mais macia \u00e9 melhor. O Tipo 440C a 55 HRC \u00e9 a entrada martens\u00edtica mais forte, com 125 MPa, o que corresponde \u00e0 sua reputa\u00e7\u00e3o como a\u00e7o ferramenta inoxid\u00e1vel para contato deslizante. O S42010 n\u00e3o engripou a 50 HRC, e o valor de dureza sozinho n\u00e3o teria previsto isso.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os graus de endurecimento por precipita\u00e7\u00e3o seguem sua temperatura de envelhecimento em vez de seu teor de liga. S45500 perde limite de forma constante \u00e0 medida que a temperatura de envelhecimento aumenta, de 90 MPa a 510 C para 59 MPa a 566 C e 28 MPa a 621 C, e S45000 faz o mesmo, de 69 MPa para 14 MPa. Uma pe\u00e7a reenvelhecida a quente para ganhar ductilidade abre m\u00e3o da resist\u00eancia ao engripamento ao faz\u00ea-lo.<\/p>\n\n\n\n<h2 id=\"h-one-design-assumption-that-does-not-survive-the-data\" class=\"wp-block-heading\">Uma premissa de projeto que n\u00e3o resiste aos dados<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Uma regra pr\u00e1tica comum \u00e9 que uma grande diferen\u00e7a de dureza entre duas pe\u00e7as acopladas previne o engripamento. Os dados de desgaste publicados n\u00e3o sustentam isso. Testados contra seis ligas de contraface diferentes, o tipo 440C a 57 HRC e o S21800 a 95 HRB foram boas escolhas independentemente da dureza do material contra o qual deslizaram. A escolha da melhor liga, e n\u00e3o o tamanho da diferen\u00e7a de dureza, determina o resultado. Dentro de um mesmo grau, a dureza ainda importa, e o mesmo ensaio mostra o tipo 440C perdendo 0,7 mm3 a 56 HRC e 44,1 mm3 a 26,5 HRC, portanto, uma vez escolhido o grau, o tratamento de endurecimento n\u00e3o \u00e9 opcional.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os graus austen\u00edticos que endurecem por deforma\u00e7\u00e3o mais rapidamente tamb\u00e9m resistem melhor ao desgaste adesivo, e \u00e9 por isso que S20161 e S21800 ficam no topo do ranking de desgaste adesivo no ensaio de cilindros cruzados e por que o tipo martens\u00edtico 410 a 24,5 HRC fica na base. O mesmo ranking coloca um a\u00e7o ferramenta comum na frente do grupo.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Material<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza<\/th><th class=\"has-text-align-left\" data-align=\"left\">A 105 rev\/min<\/th><th class=\"has-text-align-left\" data-align=\"left\">A 415 rev\/min<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">a\u00e7o ferramenta D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">61 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.46<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.34<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AISI 4337<\/td><td class=\"has-text-align-left\" data-align=\"left\">52 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.73<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.48<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Stellite 6B<\/td><td class=\"has-text-align-left\" data-align=\"left\">48 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.27<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A\u00e7o Mn Hadfield<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.41<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Bronze Al (10,5%)<\/td><td class=\"has-text-align-left\" data-align=\"left\">87 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.52<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Alum\u00ednio Tipo 6061-T6<\/td><td class=\"has-text-align-left\" data-align=\"left\">59 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">21.15<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AISI 4130<\/td><td class=\"has-text-align-left\" data-align=\"left\">47 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.44<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.80<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Astralloy V<\/td><td class=\"has-text-align-left\" data-align=\"left\">46 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">213.58<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.22<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 440C<\/td><td class=\"has-text-align-left\" data-align=\"left\">57 HRC<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.81<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.54<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S21800<\/td><td class=\"has-text-align-left\" data-align=\"left\">95 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.79<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.58<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 201<\/td><td class=\"has-text-align-left\" data-align=\"left\">90 HRB<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.95<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.68<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Ranking relativo de resist\u00eancia ao desgaste adesivo de materiais trabalhados, reproduzido do ASM Handbook, Volume 18. A perda de peso \u00e9 medida em miligramas por mil ciclos no ensaio de cilindros cruzados, ASTM G83, a 71 N. A 61 HRC, a melhor entrada da tabela \u00e9 o <a href=\"https:\/\/aobosteel.com\/pt\/d2-steel-properties\/\">a\u00e7o ferramenta D2<\/a>, \u00e0 frente da liga de revestimento duro \u00e0 base de cobalto na terceira linha.<\/em><\/p>\n\n\n\n<h2 id=\"h-temperature-moves-the-answer\" class=\"wp-block-heading\">A temperatura muda a resposta<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O desgaste adesivo n\u00e3o \u00e9 uma propriedade fixa de um par, porque tanto o filme de \u00f3xido quanto a tens\u00e3o de escoamento mudam com a temperatura. S21800 melhora \u00e0 medida que a junta opera mais quente, com a perda de volume caindo de 2,6 mm3 a 80 C para 2,2 mm3 a 315 C e 1,3 mm3 a 540 C, enquanto o tipo 304 permanece semelhante em toda a mesma faixa. O tipo 410 comporta-se de maneira oposta. A 95 HRB, perde 282,8 mm3 a 80 C, e endurec\u00ea-lo a 40 HRC reduz isso para 42,1 mm3, como com um grau martens\u00edtico, mesmo quando o limite de engripamento sugere que o revenimento mais macio \u00e9 melhor. A liga de revestimento duro \u00e0 base de cobalto na mesma s\u00e9rie come\u00e7a baixa e aumenta com a temperatura, e \u00e9 por isso que n\u00e3o \u00e9 a resposta autom\u00e1tica em toda temperatura.<\/p>\n\n\n\n<h2 id=\"h-what-to-do-about-a-stainless-tool-that-seizes\" class=\"wp-block-heading\">O que fazer com uma ferramenta inoxid\u00e1vel que agarra<\/h2>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Medida<\/th><th class=\"has-text-align-left\" data-align=\"left\">Por que funciona<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Escolha o grau a partir da lista medida<\/td><td class=\"has-text-align-left\" data-align=\"left\">A escolha do grau desloca a tens\u00e3o limiar de engripamento por um fator de vinte ou mais, portanto \u00e9 a primeira decis\u00e3o e n\u00e3o a \u00faltima.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Torne o par dissimilar<\/td><td class=\"has-text-align-left\" data-align=\"left\">Uma pe\u00e7a inoxid\u00e1vel operando contra uma fam\u00edlia de materiais diferente elimina completamente o pior do caso de desgaste por ader\u00eancia entre materiais iguais.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o confie no encruamento a frio<\/td><td class=\"has-text-align-left\" data-align=\"left\">O trefilamento a frio de um a\u00e7o austen\u00edtico aumenta sua dureza e reduz sua resist\u00eancia ao desgaste por ader\u00eancia ao mesmo tempo, o que \u00e9 o oposto do que o valor de dureza sugere.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Mantenha a superf\u00edcie retificada e livre de detritos<\/td><td class=\"has-text-align-left\" data-align=\"left\">Os valores limite publicados s\u00e3o medidos em acabamento retificado sem lubrifica\u00e7\u00e3o, portanto uma superf\u00edcie rasgada ou limada \u00e0 m\u00e3o fica abaixo deles.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Lubrifique onde a aplica\u00e7\u00e3o permite<\/td><td class=\"has-text-align-left\" data-align=\"left\">Um filme de qualquer tipo separa as asperezas que de outra forma se soldariam a frio, e o desgaste adesivo \u00e9 o mecanismo que esse filme interrompe.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Observe a temperatura de servi\u00e7o<\/td><td class=\"has-text-align-left\" data-align=\"left\">Os graus austen\u00edticos mant\u00eam ou melhoram sua resist\u00eancia ao desgaste adesivo \u00e0 medida que a junta opera mais quente, enquanto as ligas endurec\u00edveis a perdem.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Medidas contra o desgaste por ader\u00eancia em ferramentas de a\u00e7o inoxid\u00e1vel e pe\u00e7as conjugadas, do ASM Handbook, Volume 18. Os m\u00e9todos de ensaio publicados por tr\u00e1s da tabela s\u00e3o o ensaio de triagem de bot\u00e3o sobre bloco e, para conex\u00f5es roscadas, um ensaio de montagem e desmontagem na conex\u00e3o real.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Quando a pe\u00e7a \u00e9 de a\u00e7o ferramenta e n\u00e3o de inoxid\u00e1vel, o mesmo mecanismo determina o grau, e a resposta est\u00e1 apresentada em <a href=\"https:\/\/aobosteel.com\/pt\/adhesive-wear-resistant-tool-steels\/\">a\u00e7os ferramenta resistentes ao desgaste adesivo<\/a>. Os dois a\u00e7os ferramenta inoxid\u00e1veis que carregam esses dados em uma ferramentaria s\u00e3o o <a href=\"https:\/\/aobosteel.com\/pt\/440c-stainless-steel\/\">a\u00e7o inoxid\u00e1vel 440C<\/a>, o limite mais alto da fam\u00edlia martens\u00edtica, e o <a href=\"https:\/\/aobosteel.com\/pt\/420-stainless-steel\/\">a\u00e7o inoxid\u00e1vel 420<\/a>, que precisa do revenido correto para dar seu melhor resultado.<\/p>\n\n\n\n<h2 id=\"h-grades-and-stock\" class=\"wp-block-heading\">Graus e estoque<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O a\u00e7o ferramenta inoxid\u00e1vel \u00e9 comprado por duas propriedades ao mesmo tempo, e o desgaste ou engripamento \u00e9 apenas a primeira. A <a href=\"https:\/\/aobosteel.com\/pt\/stainless-steel-corrosion-resistance-chart\/\">tabela de resist\u00eancia \u00e0 corros\u00e3o de a\u00e7os inoxid\u00e1veis<\/a>\u00a0abrange a corros\u00e3o, a <a href=\"https:\/\/aobosteel.com\/pt\/stainless-steel-composition-chart\/\">tabela de composi\u00e7\u00e3o do a\u00e7o inoxid\u00e1vel<\/a> abrange a composi\u00e7\u00e3o, e a <a href=\"https:\/\/aobosteel.com\/pt\/stainless-steel-sensitization\/\">sensibiliza\u00e7\u00e3o do a\u00e7o inoxid\u00e1vel<\/a> abrange o que o calor faz ao cromo em servi\u00e7o.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Se o dano for uma mancha ou pite em vez de uma superf\u00edcie rasgada, o mecanismo \u00e9 diferente, e o diagn\u00f3stico est\u00e1 na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-pitting-corrosion\/\">corros\u00e3o por pites em a\u00e7o ferramenta<\/a>, com o caso de fresta na <a href=\"https:\/\/aobosteel.com\/pt\/mold-steel-crevice-corrosion\/\">corros\u00e3o por fresta em a\u00e7o para molde<\/a>. Onde a superf\u00edcie rasgou porque duas pe\u00e7as estavam sofrendo fretting em vez de deslizamento, o padr\u00e3o \u00e9 descrito no <a href=\"https:\/\/aobosteel.com\/pt\/fretting-wear-tool-steel\/\">desgaste por fretting em ferramentaria<\/a>, e onde um molde falhou por um motivo diferente da ader\u00eancia da pe\u00e7a de trabalho a ele, a lista de mecanismos est\u00e1 no <a href=\"https:\/\/aobosteel.com\/pt\/die-wear-and-failure-mechanisms\/\">desgaste de matrizes e mecanismos de falha<\/a>.<\/p>\n\n\n\n<h3 id=\"h-before-you-use-these-values\" class=\"wp-block-heading\">Antes de usar esses valores<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Esta p\u00e1gina \u00e9 um resumo de refer\u00eancia de pr\u00e1ticas publicadas e n\u00e3o \u00e9 uma especifica\u00e7\u00e3o da Aobo Steel. Os limites e valores de desgaste s\u00e3o reproduzidos das tabelas de origem e foram medidos em corpos de prova de laborat\u00f3rio preparados, portanto acabamento superficial, ajuste, lubrifica\u00e7\u00e3o e a geometria de contato real ir\u00e3o alter\u00e1-los. A sele\u00e7\u00e3o de grau para um trabalho de ferramentaria inoxid\u00e1vel \u00e9 confirmada no trabalho.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Fonte: ASM Handbook, Volume 18, Friction, Lubrication, and Wear Technology, ASM International, 1992.<\/p>","protected":false},"excerpt":{"rendered":"<p>Galling of Stainless Steels and How Much Stress It Takes Galling is the cold welding of microscopic high points between two sliding surfaces, and it&#8217;s why a stainless part that ran freely in the workshop seizes on the machine. All five families of stainless steel are susceptible, including the martensitic grades a tool shop buys [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-21355","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Galling of Stainless Steels: Threshold Stress Data<\/title>\n<meta name=\"description\" content=\"The threshold galling stress of every stainless family, the ranking for adhesive wear, and the two galling assumptions the measured data do not support.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/galling-of-stainless-tool-steels\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Galling of Stainless Steels and How Much Stress It Takes\" \/>\n<meta property=\"og:description\" content=\"The threshold galling stress of every stainless family, the ranking for adhesive wear, and the two galling assumptions the measured data do not support.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/galling-of-stainless-tool-steels\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-19T14:51:26+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"9 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Galling of Stainless Steels and How Much Stress It Takes\",\"datePublished\":\"2026-10-08T10:49:47+00:00\",\"dateModified\":\"2026-10-19T14:51:26+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/\"},\"wordCount\":1669,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/\",\"name\":\"Galling of Stainless Steels: Threshold Stress Data\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-08T10:49:47+00:00\",\"dateModified\":\"2026-10-19T14:51:26+00:00\",\"description\":\"The threshold galling stress of every stainless family, the ranking for adhesive wear, and the two galling assumptions the measured data do not support.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/galling-of-stainless-tool-steels\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Galling of Stainless Steels and How Much Stress It Takes\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Galling de a\u00e7os inoxid\u00e1veis: dados de tens\u00e3o limite","description":"A tens\u00e3o limite de engripamento de cada fam\u00edlia de a\u00e7o inoxid\u00e1vel, a classifica\u00e7\u00e3o para desgaste adesivo e as duas premissas de engripamento que os dados medidos n\u00e3o sustentam.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/galling-of-stainless-tool-steels\/","og_locale":"pt_BR","og_type":"article","og_title":"Galling of Stainless Steels and How Much Stress It Takes","og_description":"The threshold galling stress of every stainless family, the ranking for adhesive wear, and the two galling assumptions the measured data do not support.","og_url":"https:\/\/aobosteel.com\/pt\/galling-of-stainless-tool-steels\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-19T14:51:26+00:00","twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"9 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Galling of Stainless Steels and How Much Stress It Takes","datePublished":"2026-10-08T10:49:47+00:00","dateModified":"2026-10-19T14:51:26+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/"},"wordCount":1669,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/","url":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/","name":"Galling de a\u00e7os inoxid\u00e1veis: dados de tens\u00e3o limite","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-08T10:49:47+00:00","dateModified":"2026-10-19T14:51:26+00:00","description":"A tens\u00e3o limite de engripamento de cada fam\u00edlia de a\u00e7o inoxid\u00e1vel, a classifica\u00e7\u00e3o para desgaste adesivo e as duas premissas de engripamento que os dados medidos n\u00e3o sustentam.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/galling-of-stainless-tool-steels\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Galling of Stainless Steels and How Much Stress It Takes"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Galling of Stainless Steels and How Much Stress It Takes Galling is the cold welding of microscopic high points between two sliding surfaces, and it&#8217;s why a stainless part that ran freely in the workshop seizes on the machine. All five families of stainless steel are susceptible, including the martensitic grades a tool shop buys&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Galling of Stainless Steels and How Much Stress It Takes Galling is the cold welding of microscopic high points between two sliding surfaces, and it&#8217;s why a stainless part that ran freely in the workshop seizes on the machine. All five families of stainless steel are susceptible, including the martensitic grades a tool shop buys&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21355","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=21355"}],"version-history":[{"count":6,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21355\/revisions"}],"predecessor-version":[{"id":23703,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21355\/revisions\/23703"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=21355"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}