{"id":21191,"date":"2026-10-07T21:21:52","date_gmt":"2026-10-07T13:21:52","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=21191"},"modified":"2026-11-12T20:16:33","modified_gmt":"2026-11-12T12:16:33","slug":"stainless-steel-sensitization","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/stainless-steel-sensitization\/","title":{"rendered":"Sensibiliza\u00e7\u00e3o e Corros\u00e3o Intergranular em A\u00e7o Ferramenta Inoxid\u00e1vel"},"content":{"rendered":"<h1 class=\"wp-block-heading\">Sensibiliza\u00e7\u00e3o e Corros\u00e3o Intergranular em A\u00e7o Ferramenta Inoxid\u00e1vel<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">Um a\u00e7o ferramenta inoxid\u00e1vel que falhou ao longo de seus contornos de gr\u00e3o geralmente passou em todas as verifica\u00e7\u00f5es do desenho. O grau est\u00e1 correto, a dureza est\u00e1 correta e a superf\u00edcie estava limpa. O que deu errado \u00e9 uma etapa de tratamento t\u00e9rmico que conduziu o a\u00e7o atrav\u00e9s de uma faixa de temperatura, ou o manteve l\u00e1 por tempo demais, e deixou o metal ao lado de cada contorno de gr\u00e3o com falta do cromo que torna o a\u00e7o inoxid\u00e1vel em primeiro lugar. Esta p\u00e1gina aborda quando isso acontece, o que custa em taxa de corros\u00e3o e como o resultado \u00e9 testado e aceito.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Por que um a\u00e7o inoxid\u00e1vel pode corroer ao longo de seus contornos de gr\u00e3o<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O cromo \u00e9 o que torna um a\u00e7o inoxid\u00e1vel. Acima de cerca de 1035 C (1900 F) os carbonetos de cromo em um a\u00e7o inoxid\u00e1vel austen\u00edtico s\u00e3o completamente dissolvidos, ent\u00e3o o cromo fica em solu\u00e7\u00e3o s\u00f3lida e est\u00e1 dispon\u00edvel para construir o filme passivo que protege a superf\u00edcie. Resfrie o a\u00e7o lentamente a partir dessa temperatura, ou reaque\u00e7a-o para 425 a 815 C (800 a 1500 F), e os carbonetos precipitam nos contornos de gr\u00e3o. Cada carboneto carrega mais cromo do que a matriz ao redor, ent\u00e3o a precipita\u00e7\u00e3o drena o cromo de uma zona estreita em ambos os lados de cada contorno. O cromo difunde lentamente nessas temperaturas, ent\u00e3o a zona empobrecida permanece onde est\u00e1. O a\u00e7o ent\u00e3o est\u00e1 sensibilizado, o que significa que os contornos corroem preferencialmente enquanto os pr\u00f3prios gr\u00e3os permanecem brilhantes.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A fonte quantifica o quanto isso importa. Em \u00e1cido sulf\u00farico 50% em ebuli\u00e7\u00e3o com sulfato f\u00e9rrico adicionado, ligas de ferro-cromo mostram uma taxa de corros\u00e3o que cai acentuadamente \u00e0 medida que o teor de cromo aumenta, e o teste \u00e9 mais sens\u00edvel entre 12 e 18% Cr. Essa \u00e9 exatamente a faixa de cromo que os a\u00e7os ferramenta inoxid\u00e1veis martens\u00edticos ocupam, ent\u00e3o uma perda de cromo no contorno n\u00e3o \u00e9 um efeito pequeno no ambiente que esse teste representa. Com os n\u00edveis de cromo mais baixos o filme passivo \u00e9 mais sol\u00favel no \u00e1cido, ent\u00e3o mais metal tem que se dissolver para reparar o filme e a taxa medida sobe.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Onde o a\u00e7o se situa no ciclo<\/th><th class=\"has-text-align-left\" data-align=\"left\">O que os carbonetos fazem<\/th><th class=\"has-text-align-left\" data-align=\"left\">O que isso deixa no a\u00e7o<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Acima de cerca de 1035 C (1900 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">Os carbonetos de cromo s\u00e3o completamente dissolvidos na austenita<\/td><td class=\"has-text-align-left\" data-align=\"left\">Uma estrutura tratada em solu\u00e7\u00e3o limpa sem cromo retido nos contornos de gr\u00e3o<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Resfriamento lento a partir de acima de 1035 C, ou qualquer reaquecimento para 425 a 815 C (800 a 1500 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">Os carbonetos de cromo precipitam nos contornos de gr\u00e3o, e cada carboneto cont\u00e9m mais cromo do que a matriz ao redor<\/td><td class=\"has-text-align-left\" data-align=\"left\">A matriz ao lado de cada contorno fica empobrecida em cromo e o a\u00e7o \u00e9 sensibilizado<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Cerca de 675 C (1250 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">Taxa m\u00e1xima de precipita\u00e7\u00e3o de carboneto de cromo<\/td><td class=\"has-text-align-left\" data-align=\"left\">O pior ponto da janela, e \u00e9 uma temperatura normal de al\u00edvio de tens\u00f5es para a\u00e7os carbono e de baixa liga<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Mantido abaixo de cerca de 425 C (800 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">Os carbonetos n\u00e3o precipitam de forma alguma<\/td><td class=\"has-text-align-left\" data-align=\"left\">Um resfriamento r\u00e1pido atrav\u00e9s deste n\u00edvel deixa o a\u00e7o imune \u00e0 corros\u00e3o intergranular<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A zona afetada pelo calor de uma solda<\/td><td class=\"has-text-align-left\" data-align=\"left\">Parte da zona permanece dentro da faixa de precipita\u00e7\u00e3o tempo suficiente para formar carbonetos enquanto a pr\u00f3pria solda esfria rapidamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">Decaimento de solda, que \u00e9 o caso cl\u00e1ssico de campo de sensibiliza\u00e7\u00e3o<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>A janela de sensibiliza\u00e7\u00e3o conforme a fonte a define. O a\u00e7o \u00e9 seguro acima da temperatura de solu\u00e7\u00e3o e seguro abaixo da faixa de precipita\u00e7\u00e3o, e o risco est\u00e1 inteiramente no resfriamento e em qualquer tratamento t\u00e9rmico posterior que retorne para 425 a 815 C. Compilado da se\u00e7\u00e3o de corros\u00e3o intergranular do artigo.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O resfriamento r\u00e1pido atrav\u00e9s de cerca de 425 C (800 F) \u00e9 a resposta no forno, porque os carbonetos nunca t\u00eam tempo de se formar. A armadilha \u00e9 a etapa ap\u00f3s o endurecimento. O al\u00edvio de tens\u00f5es de a\u00e7os carbono e de baixa liga \u00e9 comumente feito a cerca de 675 C, que tamb\u00e9m \u00e9 a temperatura de pico de precipita\u00e7\u00e3o de carbonetos em a\u00e7o inoxid\u00e1vel, ent\u00e3o uma pe\u00e7a inoxid\u00e1vel compartilhando uma carga com pe\u00e7as de a\u00e7o carbono em um ciclo de al\u00edvio de tens\u00f5es pode ser sensibilizada por um tratamento que nunca foi direcionado a ela. A soldagem faz a mesma coisa em menor escala, porque a zona afetada pelo calor passa pela faixa de precipita\u00e7\u00e3o enquanto a pr\u00f3pria po\u00e7a de solda esfria r\u00e1pido o suficiente para evit\u00e1-la.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">O que o revenimento faz a um a\u00e7o ferramenta inoxid\u00e1vel<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Os graus inoxid\u00e1veis martens\u00edticos usados para cutelaria, moldes e pe\u00e7as de desgaste endurecem porque a t\u00eampera produz martensita, e a martensita tem que ser revenida para restaurar a ductilidade. Essa etapa de revenimento \u00e9 em si um reaquecimento para uma faixa de temperatura onde os carbonetos se formam, ent\u00e3o a resist\u00eancia \u00e0 corros\u00e3o de um a\u00e7o inoxid\u00e1vel martens\u00edtico endurecido e revenido depende de como foi revenido e n\u00e3o apenas de sua an\u00e1lise. A fonte registra a medi\u00e7\u00e3o relacionada para um a\u00e7o inoxid\u00e1vel ferr\u00edtico, uma temperatura de in\u00edcio de martensita de 176 C (349 F) para um a\u00e7o com 17% Cr com a transforma\u00e7\u00e3o 90% completa a 93 C (199 F), uma temperatura de in\u00edcio de menos 160 C para um a\u00e7o com 21% Cr, e nenhuma martensita em ligas temperadas com 25% Cr. A martensita n\u00e3o revenida remove tenacidade e ductilidade, e tamb\u00e9m corr\u00f3i mais r\u00e1pido do que a estrutura ao seu redor.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A raz\u00e3o pela qual corr\u00f3i mais r\u00e1pido vale a pena levar para uma discuss\u00e3o com um cliente. Quando ligas de ferro-cromo se separam em ferrita e austenita em alta temperatura, as duas fases n\u00e3o cont\u00eam a mesma quantidade de cromo, e a austenita \u00e9 a mais pobre das duas. A martensita que se forma a partir dessa austenita herda a composi\u00e7\u00e3o mais pobre, ent\u00e3o tem menos cromo do que a ferrita ao seu lado e se dissolve primeiro no teste de \u00e1cido sulf\u00farico em ebuli\u00e7\u00e3o. A fonte relata exatamente esse comportamento para a martensita no tipo 430, e observa que o teste \u00e9 insens\u00edvel \u00e0 mesma diferen\u00e7a em n\u00edveis mais altos de cromo, raz\u00e3o pela qual nenhum ataque preferencial apareceu na austenita formada no tipo 446. Em termos simples, a fase com menor teor de cromo \u00e9 a fase que corr\u00f3i primeiro, independentemente do que o nome do grau diga no certificado.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">As fases secund\u00e1rias que retiram o cromo<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Os carbonetos s\u00e3o apenas os mais conhecidos das fases que se formam quando o a\u00e7o inoxid\u00e1vel \u00e9 mantido em temperatura. A fonte lista o conjunto completo com a faixa em que cada um aparece, e eles se sobrep\u00f5em de uma forma que importa para um cronograma de tratamento t\u00e9rmico. A fase sigma e a fase chi formam-se em aproximadamente 550 a 1050 C (1020 a 1920 F) e 600 a 900 C (1110 a 1650 F) respectivamente, e ambas reduzem a resist\u00eancia \u00e0 corros\u00e3o e custam ductilidade e tenacidade. Alfa linha \u00e9 uma fase rica em cromo que aparece a uma temperatura muito mais baixa, 350 a 550 C (660 a 1020 F), e embora tenha pouco efeito na resist\u00eancia \u00e0 corros\u00e3o sua forma\u00e7\u00e3o \u00e9 a raz\u00e3o para a perda de tenacidade conhecida como fragiliza\u00e7\u00e3o a 475 C.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Fase<\/th><th class=\"has-text-align-left\" data-align=\"left\">S\u00edmbolo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">F\u00f3rmula<\/th><th class=\"has-text-align-left\" data-align=\"left\">Faixa, C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Faixa, F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Carboneto de cromo<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">M7C3<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Cr,Fe,Mo)7C3<\/td><td class=\"has-text-align-left\" data-align=\"left\">950 a 1050<\/td><td class=\"has-text-align-left\" data-align=\"left\">1740 a 1920<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Carboneto de cromo<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">M23C6<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Cr,Fe,Mo)23C6<\/td><td class=\"has-text-align-left\" data-align=\"left\">600 a 950<\/td><td class=\"has-text-align-left\" data-align=\"left\">1110 a 1740<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Carboneto de cromo<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">M6C<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Cr,Fe,MoNb)6C<\/td><td class=\"has-text-align-left\" data-align=\"left\">700 a 950<\/td><td class=\"has-text-align-left\" data-align=\"left\">1290 a 1740<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitreto de cromo<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">M2N<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Cr,Fe)2N<\/td><td class=\"has-text-align-left\" data-align=\"left\">650 a 950<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200 a 1740<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitreto de Fe-Mo<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">M5N<\/td><td class=\"has-text-align-left\" data-align=\"left\">Fe7Mo13N4<\/td><td class=\"has-text-align-left\" data-align=\"left\">550 a 600<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020 a 1110<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitreto de Nb-Cr<\/td><td class=\"has-text-align-left\" data-align=\"left\">Z<\/td><td class=\"has-text-align-left\" data-align=\"left\">MN<\/td><td class=\"has-text-align-left\" data-align=\"left\">(NbCr)N<\/td><td class=\"has-text-align-left\" data-align=\"left\">700 a 1000<\/td><td class=\"has-text-align-left\" data-align=\"left\">1290 a 1830<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Carbonitreto de ni\u00f3bio<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">MC<\/td><td class=\"has-text-align-left\" data-align=\"left\">Nb(CN)<\/td><td class=\"has-text-align-left\" data-align=\"left\">700 ao ponto de fus\u00e3o<\/td><td class=\"has-text-align-left\" data-align=\"left\">1290 ao ponto de fus\u00e3o<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Sigma<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u03c3<\/td><td class=\"has-text-align-left\" data-align=\"left\">AB<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Fe,Cr,Mo,Ni)<\/td><td class=\"has-text-align-left\" data-align=\"left\">550 a 1050<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020 a 1920<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Chi<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u03c7<\/td><td class=\"has-text-align-left\" data-align=\"left\">A48B10<\/td><td class=\"has-text-align-left\" data-align=\"left\">Fe36Cr12Mo10 sobre (FeNi)36Cr18(TiMo)4<\/td><td class=\"has-text-align-left\" data-align=\"left\">600 a 900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1110 a 1650<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Alfa linha<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u03b1\u2032<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">CrFe com 61 a 83% Cr<\/td><td class=\"has-text-align-left\" data-align=\"left\">350 a 550<\/td><td class=\"has-text-align-left\" data-align=\"left\">660 a 1020<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Laves<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u03b7<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2B<\/td><td class=\"has-text-align-left\" data-align=\"left\">(FeCr)2(Mo,Nb,Ti,Si)<\/td><td class=\"has-text-align-left\" data-align=\"left\">550 a 900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020 a 1650<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">R<\/td><td class=\"has-text-align-left\" data-align=\"left\">R<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Fe,Mo,Cr,Ni)<\/td><td class=\"has-text-align-left\" data-align=\"left\">550 a 650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020 a 1200<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tau<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u03c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><td class=\"has-text-align-left\" data-align=\"left\">550 a 650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020 a 1200<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fases secund\u00e1rias em a\u00e7os inoxid\u00e1veis com a faixa de temperatura na qual cada uma se forma. O c\u00f3digo de tipo na fonte \u00e9 A para austen\u00edtico, D para duplex e F para ferr\u00edtico. Fonte, Tabela 8 do artigo.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Duas das entradas dessa tabela merecem uma nota para o trabalho com a\u00e7os-ferramenta. Os carbonetos de cromo M7C3 e M23C6 delimitam a faixa de revenimento entre si, com o M23C6 se formando de cerca de 600 a 950 C (1110 a 1740 F) e o M7C3 acima disso, de modo que qualquer cronograma de revenimento nessa faixa \u00e9, por defini\u00e7\u00e3o, um cronograma de precipita\u00e7\u00e3o de carbonetos. E a fonte \u00e9 expl\u00edcita que o nitrog\u00eanio \u00e9 o que permite que os graus inoxid\u00e1veis altamente ligados sejam usados na condi\u00e7\u00e3o como soldado, porque o nitrog\u00eanio retarda a precipita\u00e7\u00e3o das fases intermet\u00e1licas. Onde um grau \u00e9 estabilizado com tit\u00e2nio ou ni\u00f3bio, o problema do carboneto de cromo \u00e9 amplamente eliminado, porque esses elementos formam carbonetos mais est\u00e1veis que o cromo acima de cerca de 815 C (1500 F). Uma ressalva acompanha isso, e a fonte a declara diretamente. O carboneto de tit\u00e2nio pode ele pr\u00f3prio ser atacado por \u00e1cido n\u00edtrico, ent\u00e3o um a\u00e7o estabilizado com tit\u00e2nio n\u00e3o \u00e9 automaticamente a resposta certa em um meio altamente oxidante.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">O que a fase sigma custa em taxa de corros\u00e3o<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Um conjunto de medi\u00e7\u00f5es na fonte demonstra o ponto melhor que qualquer descri\u00e7\u00e3o. Uma \u00fanica liga Fe-47Cr foi tratada termicamente de modo que fosse inteiramente ferrita ou inteiramente fase sigma, e as duas estruturas foram ent\u00e3o testadas lado a lado nas mesmas solu\u00e7\u00f5es. A tabela abaixo fornece ambas as taxas e a raz\u00e3o que a pr\u00f3pria fonte reporta. Sob condi\u00e7\u00f5es redutoras, a fase sigma corr\u00f3i entre duas e cinco vezes mais r\u00e1pido que a ferrita. Sob condi\u00e7\u00f5es oxidantes, a raz\u00e3o vai a 10, 24 e 42 dependendo do \u00e1cido, e no teste de pitting com cloreto f\u00e9rrico a ferrita n\u00e3o corr\u00f3i de forma alguma, enquanto a fase sigma perde 2,5 g\/dm2\/d.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Solu\u00e7\u00e3o<\/th><th class=\"has-text-align-left\" data-align=\"left\">Ferrita, g\/dm2\/d<\/th><th class=\"has-text-align-left\" data-align=\"left\">Fase sigma, g\/dm2\/d<\/th><th class=\"has-text-align-left\" data-align=\"left\">Raz\u00e3o<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"4\">Condi\u00e7\u00f5es redutoras<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10% HCl, fervente<\/td><td class=\"has-text-align-left\" data-align=\"left\">1461<\/td><td class=\"has-text-align-left\" data-align=\"left\">7543<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10% H2SO4, fervente<\/td><td class=\"has-text-align-left\" data-align=\"left\">2939<\/td><td class=\"has-text-align-left\" data-align=\"left\">7422<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50% H2SO4, fervente<\/td><td class=\"has-text-align-left\" data-align=\"left\">5088<\/td><td class=\"has-text-align-left\" data-align=\"left\">5280<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.04<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"4\">Condi\u00e7\u00f5es oxidantes<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50% H2SO4 + Fe2(SO4)3, fervente<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0195<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.196<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50% H2SO4 + CuSO4, fervente<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0170<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.415<\/td><td class=\"has-text-align-left\" data-align=\"left\">24<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">65% HNO3, fervente<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0205<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.861<\/td><td class=\"has-text-align-left\" data-align=\"left\">42<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">HNO3 + HF a 65 C (150 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"4\">Condi\u00e7\u00f5es de pitting<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10% FeCl3.6H2O \u00e0 temperatura ambiente<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2026<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>A taxa de corros\u00e3o da fase sigma em rela\u00e7\u00e3o \u00e0 taxa de corros\u00e3o da ferrita na mesma liga Fe-47Cr, em oito solu\u00e7\u00f5es e um teste de pitting. A coluna de raz\u00e3o \u00e9 o valor da pr\u00f3pria fonte. Fonte, Tabela 4 do artigo.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A fonte tira disso uma conclus\u00e3o que vale repetir, porque n\u00e3o \u00e9 a intuitiva. A fase sigma n\u00e3o precisa de um mecanismo de deple\u00e7\u00e3o de cromo para explicar por que reduz a resist\u00eancia \u00e0 corros\u00e3o. \u00c9 simplesmente uma estrutura que corr\u00f3i mais r\u00e1pido que a ferrita por conta pr\u00f3pria. Isso muda a quest\u00e3o pr\u00e1tica. Uma rede de segunda fase nos contornos de gr\u00e3o \u00e9 um problema porque \u00e9 um caminho cont\u00ednuo de material menos resistente, e uma col\u00f4nia isolada da mesma fase \u00e9 muito menos problem\u00e1tica, ent\u00e3o a forma do que se formou pode importar tanto quanto quanto se formou. O trabalho a frio acelera a precipita\u00e7\u00e3o da fase sigma, e adi\u00e7\u00f5es de n\u00edquel at\u00e9 cerca de 2% a aceleram ainda mais, enquanto teores mais altos de n\u00edquel a retardam novamente.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Como a sensitiza\u00e7\u00e3o \u00e9 testada e aceita<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O objetivo desses testes n\u00e3o \u00e9 reproduzir um ambiente de servi\u00e7o. \u00c9 responder a uma quest\u00e3o mais restrita, se o material fornecido est\u00e1 na condi\u00e7\u00e3o metal\u00fargica que foi encomendada, raz\u00e3o pela qual s\u00e3o usados como testes de aceita\u00e7\u00e3o e n\u00e3o como dados de projeto. Para a\u00e7os inoxid\u00e1veis austen\u00edticos, a norma \u00e9 a ASTM A 262, que cont\u00e9m seis pr\u00e1ticas. A Pr\u00e1tica A \u00e9 um ataque eletrol\u00edtico com \u00e1cido ox\u00e1lico, um teste de triagem que leva minutos e \u00e9 avaliado examinando a microestrutura atacada quanto \u00e0 sensitiza\u00e7\u00e3o por carboneto de cromo. A Pr\u00e1tica B roda 120 horas em sulfato f\u00e9rrico fervente mais \u00e1cido sulf\u00farico e reporta uma taxa de perda de peso. A Pr\u00e1tica C roda 240 horas em \u00e1cido n\u00edtrico 65% fervente e detecta fase sigma bem como carbonetos. A Pr\u00e1tica E roda 24 horas em sulfato de cobre 6% fervente mais \u00e1cido sulf\u00farico 10% com cobre met\u00e1lico adicionado, e \u00e9 avaliada dobrando o corpo de prova e procurando fissuras. A Pr\u00e1tica F \u00e9 um teste fervente de 120 horas em sulfato de cobre mais \u00e1cido sulf\u00farico 50% com cobre presente, voltado para graus contendo molibd\u00eanio.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A\u00e7os inoxid\u00e1veis ferr\u00edticos s\u00e3o tratados pela ASTM A 763, que segue a mesma forma da A 262 com um ataque ox\u00e1lico e tr\u00eas testes de imers\u00e3o em \u00e1cido, e ligas de cromo-n\u00edquel forjadas ricas em n\u00edquel pela ASTM G 28. A \u00fanica diferen\u00e7a estrutural na A 763 \u00e9 que as exposi\u00e7\u00f5es \u00e1cidas s\u00e3o avaliadas sob o microsc\u00f3pio, e a presen\u00e7a ou aus\u00eancia de queda de gr\u00e3os torna-se o crit\u00e9rio de aceita\u00e7\u00e3o. A tabela abaixo re\u00fane os crit\u00e9rios de aceita\u00e7\u00e3o que a fonte tabula, incluindo o tratamento sensitizante que \u00e9 aplicado primeiro, porque um limite sem o tratamento que o produziu n\u00e3o \u00e9 uma especifica\u00e7\u00e3o utiliz\u00e1vel.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Liga<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tratamento sensitizante<\/th><th class=\"has-text-align-left\" data-align=\"left\">Teste<\/th><th class=\"has-text-align-left\" data-align=\"left\">Exposi\u00e7\u00e3o, h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa m\u00e1xima admiss\u00edvel, mm\/m\u00eas (mils\/m\u00eas)<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">Nenhum<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sulfato f\u00e9rrico, A 262-B<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.1 (4)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">1 h a 675 C (1250 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u00c1cido n\u00edtrico, A 262-C<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 (2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 309S<\/td><td class=\"has-text-align-left\" data-align=\"left\">Nenhum<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u00c1cido n\u00edtrico, A 262-C<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025 (1)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">Nenhum<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sulfato f\u00e9rrico, A 262-B<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.1 (4)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">1 h a 675 C (1250 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sulfato f\u00e9rrico, A 262-B<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.1 (4)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 317L<\/td><td class=\"has-text-align-left\" data-align=\"left\">1 h a 675 C (1250 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sulfato f\u00e9rrico, A 262-B<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.1 (4)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 321<\/td><td class=\"has-text-align-left\" data-align=\"left\">1 h a 675 C (1250 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u00c1cido n\u00edtrico, A 262-C<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 (2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tipo 347<\/td><td class=\"has-text-align-left\" data-align=\"left\">1 h a 675 C (1250 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u00c1cido n\u00edtrico, A 262-C<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 (2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20Cb-3<\/td><td class=\"has-text-align-left\" data-align=\"left\">1 h a 675 C (1250 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sulfato f\u00e9rrico, G 28-A<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 (2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">904L<\/td><td class=\"has-text-align-left\" data-align=\"left\">Nenhum<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sulfato f\u00e9rrico, G 28-A<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 (2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Incoloy 825<\/td><td class=\"has-text-align-left\" data-align=\"left\">1 h a 675 C (1250 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u00c1cido n\u00edtrico, A 262-C<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.075 (3)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">29-4-2<\/td><td class=\"has-text-align-left\" data-align=\"left\">Nenhum<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sulfato f\u00e9rrico, A 763-X<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">Sem queda significativa de gr\u00e3o<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Ensaios de avalia\u00e7\u00e3o e crit\u00e9rios de aceita\u00e7\u00e3o para ligas trabalhadas conforme a fonte os tabula, com o tratamento sensibilizante qualificante e o limite de aprova\u00e7\u00e3o para cada um. Fonte, Tabela 1 do artigo Evaluating Intergranular Corrosion.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Para uma verifica\u00e7\u00e3o em uma \u00fanica pe\u00e7a de produ\u00e7\u00e3o em vez de uma amostra de certifica\u00e7\u00e3o, a fonte descreve o ensaio de reativa\u00e7\u00e3o eletroqu\u00edmica da ASTM G 108. Um corpo de prova polido \u00e9 polarizado de sua condi\u00e7\u00e3o passiva para a faixa ativa em \u00e1cido sulf\u00farico com tiocianato de pot\u00e1ssio, e a carga que passa durante a reativa\u00e7\u00e3o est\u00e1 relacionada \u00e0 precipita\u00e7\u00e3o de carboneto de cromo nos contornos de gr\u00e3o. Os valores de refer\u00eancia que a fonte fornece s\u00e3o uma carga por unidade de \u00e1rea de contorno de gr\u00e3o abaixo de 0,1 C\/cm2 para uma microestrutura n\u00e3o sensibilizada e acima de 0,4 C\/cm2 para uma fortemente sensibilizada. Esse ensaio \u00e9 r\u00e1pido o suficiente para ser executado em uma pe\u00e7a retirada de um lote, o que as imers\u00f5es em \u00e1cido de 120 e 240 horas n\u00e3o s\u00e3o.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">O que isso significa em um pedido de a\u00e7o ferramenta<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Tr\u00eas coisas decorrem disso para quem compra ou trata termicamente um a\u00e7o-ferramenta inoxid\u00e1vel. A qu\u00edmica e o tratamento t\u00e9rmico juntos decidem a resist\u00eancia \u00e0 corros\u00e3o, portanto uma classe nunca deve ser selecionada apenas pela an\u00e1lise onde a pe\u00e7a ser\u00e1 revenida ou aliviada de tens\u00f5es. As fases secund\u00e1rias na tabela acima se sobrep\u00f5em \u00e0s faixas de revenimento das classes martens\u00edticas, ent\u00e3o a temperatura de revenimento deve ser escolhida considerando tanto a dureza quanto o requisito de corros\u00e3o. E onde a sensibiliza\u00e7\u00e3o importa, o ensaio de aceita\u00e7\u00e3o pertence \u00e0 especifica\u00e7\u00e3o de compra, juntamente com o tratamento sensibilizante qualificante, porque o limite por si s\u00f3 n\u00e3o descreve nada. O mesmo quadro metal\u00fargico do lado do tratamento t\u00e9rmico est\u00e1 em <a href=\"https:\/\/aobosteel.com\/pt\/martensitic-stainless-steel-microstructure\/\">a microestrutura do a\u00e7o inoxid\u00e1vel martens\u00edtico<\/a>, os pr\u00f3prios ciclos est\u00e3o em <a href=\"https:\/\/aobosteel.com\/pt\/440c-stainless-steel-heat-treatment\/\">Tratamento t\u00e9rmico do a\u00e7o inoxid\u00e1vel 440C<\/a> e <a href=\"https:\/\/aobosteel.com\/pt\/420-stainless-steel-heat-treatment\/\">Tratamento t\u00e9rmico de a\u00e7o inoxid\u00e1vel 420<\/a>, e o comportamento \u00e0 corros\u00e3o das classes fornecidas pela Aobo est\u00e1 representado em <a href=\"https:\/\/aobosteel.com\/pt\/stainless-steel-corrosion-resistance-chart\/\">o gr\u00e1fico de resist\u00eancia \u00e0 corros\u00e3o do a\u00e7o inoxid\u00e1vel<\/a>. As falhas em servi\u00e7o que decorrem de um tratamento t\u00e9rmico incorreto est\u00e3o em <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-size-change-in-heat-treatment\/\">Varia\u00e7\u00e3o dimensional no tratamento t\u00e9rmico<\/a> e <a href=\"https:\/\/aobosteel.com\/pt\/quench-cracking-tool-steel\/\">trincas de t\u00eampera em a\u00e7o ferramenta<\/a>, o lado da limpeza do mesmo problema de contorno est\u00e1 em <a href=\"https:\/\/aobosteel.com\/pt\/steel-inclusion-and-grain-size-measurement\/\">medi\u00e7\u00e3o de inclus\u00f5es e tamanho de gr\u00e3o<\/a> e o <a href=\"https:\/\/aobosteel.com\/pt\/steel-bar-and-billet-inspection\/\">p\u00e1gina de inspe\u00e7\u00e3o de barras e blocos de a\u00e7o<\/a>, e as pr\u00f3prias classes s\u00e3o descritas em <a href=\"https:\/\/aobosteel.com\/pt\/4cr13-stainless-steel\/\">A\u00e7o inoxid\u00e1vel 4Cr13<\/a> e <a href=\"https:\/\/aobosteel.com\/pt\/plastic-mold-steels\/\">a\u00e7os para moldes de pl\u00e1stico<\/a>. Onde um ambiente com cloreto tamb\u00e9m est\u00e1 presente, o ataque de contorno pode se transformar em trincamento, que \u00e9 o assunto de <a href=\"https:\/\/aobosteel.com\/pt\/steel-embrittlement-types\/\">os tipos de fragiliza\u00e7\u00e3o do a\u00e7o<\/a>.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Antes de agir sobre um diagn\u00f3stico de sensibiliza\u00e7\u00e3o<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Uma p\u00e1gina de refer\u00eancia, n\u00e3o \u00e9 uma especifica\u00e7\u00e3o da Aobo Steel, e as taxas e crit\u00e9rios acima s\u00e3o os valores publicados para as ligas, tratamentos e solu\u00e7\u00f5es espec\u00edficos nomeados. Um ensaio \u00e1cido acelerado classifica materiais e confirma uma condi\u00e7\u00e3o entregue, n\u00e3o prev\u00ea a vida \u00fatil em servi\u00e7o em uma planta. As faixas de temperatura s\u00e3o dadas para as fam\u00edlias de a\u00e7o inoxid\u00e1vel que a fonte estava descrevendo, e o limite exato da janela de sensibiliza\u00e7\u00e3o muda com o teor de carbono, o teor de nitrog\u00eanio e as adi\u00e7\u00f5es estabilizantes na classe \u00e0 sua frente. Trate os limites de aceita\u00e7\u00e3o como um ponto de partida para uma especifica\u00e7\u00e3o de compra que nomeie seu pr\u00f3prio tratamento qualificante, e confirme a estrutura na pe\u00e7a real antes de concluir que o tratamento t\u00e9rmico foi a causa.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Fonte: ASM Handbook, Volume 13A, Corrosion: Fundamentals, Testing, and Protection, ASM International, 2003.<\/p>","protected":false},"excerpt":{"rendered":"<p>Sensitization and Intergranular Corrosion in Stainless Tool Steel A stainless tool steel that failed along its grain boundaries usually passed every check on the drawing. The grade is right, the hardness is right, and the surface was clean. What went wrong is a heat treatment step that walked the steel through one temperature range, or [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-21191","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Sensitization and Intergranular Corrosion in Stainless Tool Steel<\/title>\n<meta name=\"description\" content=\"Chromium carbide precipitation between 425 and 815 C leaves stainless tool steel sensitized at its grain boundaries. Mechanism, secondary phases and acceptance tests.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/stainless-steel-sensitization\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Sensitization and Intergranular Corrosion in Stainless Tool Steel\" \/>\n<meta property=\"og:description\" content=\"Chromium carbide precipitation between 425 and 815 C leaves stainless tool steel sensitized at its grain boundaries. Mechanism, secondary phases and acceptance tests.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/stainless-steel-sensitization\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-11-12T12:16:33+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"13 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Sensitization and Intergranular Corrosion in Stainless Tool Steel\",\"datePublished\":\"2026-10-07T13:21:52+00:00\",\"dateModified\":\"2026-11-12T12:16:33+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/\"},\"wordCount\":2641,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/\",\"name\":\"Sensitization and Intergranular Corrosion in Stainless Tool Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-07T13:21:52+00:00\",\"dateModified\":\"2026-11-12T12:16:33+00:00\",\"description\":\"Chromium carbide precipitation between 425 and 815 C leaves stainless tool steel sensitized at its grain boundaries. Mechanism, secondary phases and acceptance tests.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Sensitization and Intergranular Corrosion in Stainless Tool Steel\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Sensibiliza\u00e7\u00e3o e Corros\u00e3o Intergranular em A\u00e7o Ferramenta Inoxid\u00e1vel","description":"A precipita\u00e7\u00e3o de carbonetos de cromo entre 425 e 815 C deixa o a\u00e7o ferramenta inoxid\u00e1vel sensitizado nos contornos de gr\u00e3o. Mecanismo, fases secund\u00e1rias e ensaios de aceita\u00e7\u00e3o.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/stainless-steel-sensitization\/","og_locale":"pt_BR","og_type":"article","og_title":"Sensitization and Intergranular Corrosion in Stainless Tool Steel","og_description":"Chromium carbide precipitation between 425 and 815 C leaves stainless tool steel sensitized at its grain boundaries. Mechanism, secondary phases and acceptance tests.","og_url":"https:\/\/aobosteel.com\/pt\/stainless-steel-sensitization\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-11-12T12:16:33+00:00","twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"13 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Sensitization and Intergranular Corrosion in Stainless Tool Steel","datePublished":"2026-10-07T13:21:52+00:00","dateModified":"2026-11-12T12:16:33+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/"},"wordCount":2641,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/","url":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/","name":"Sensibiliza\u00e7\u00e3o e Corros\u00e3o Intergranular em A\u00e7o Ferramenta Inoxid\u00e1vel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-07T13:21:52+00:00","dateModified":"2026-11-12T12:16:33+00:00","description":"A precipita\u00e7\u00e3o de carbonetos de cromo entre 425 e 815 C deixa o a\u00e7o ferramenta inoxid\u00e1vel sensitizado nos contornos de gr\u00e3o. Mecanismo, fases secund\u00e1rias e ensaios de aceita\u00e7\u00e3o.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/stainless-steel-sensitization\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Sensitization and Intergranular Corrosion in Stainless Tool Steel"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Sensitization and Intergranular Corrosion in Stainless Tool Steel A stainless tool steel that failed along its grain boundaries usually passed every check on the drawing. The grade is right, the hardness is right, and the surface was clean. What went wrong is a heat treatment step that walked the steel through one temperature range, or&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Sensitization and Intergranular Corrosion in Stainless Tool Steel A stainless tool steel that failed along its grain boundaries usually passed every check on the drawing. The grade is right, the hardness is right, and the surface was clean. What went wrong is a heat treatment step that walked the steel through one temperature range, or&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21191","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=21191"}],"version-history":[{"count":4,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21191\/revisions"}],"predecessor-version":[{"id":25300,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21191\/revisions\/25300"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=21191"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}