{"id":21119,"date":"2026-10-07T16:10:25","date_gmt":"2026-10-07T08:10:25","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=21119"},"modified":"2026-10-07T16:10:25","modified_gmt":"2026-10-07T08:10:25","slug":"tool-steel-weld-filler-metals","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/tool-steel-weld-filler-metals\/","title":{"rendered":"Metais de adi\u00e7\u00e3o para soldagem de a\u00e7o-ferramenta"},"content":{"rendered":"\n<style>\n\n:root{\n    --aobo-accent:#2563eb; --aobo-accent-dark:#1e1e2e; --aobo-blue:#0c56d0; --aobo-blue-dark:#073b91;\n    --aobo-text:#333; --aobo-muted:#888; --aobo-border:#e5e7eb; --aobo-border-dark:#ddd;\n    --aobo-stripe:#f7f7f9; --aobo-hover:#e8f0fe; --aobo-radius:8px; --aobo-radius-sm:6px;\n    --aobo-orange:#f59e0b; --aobo-fill:#e9ecef;\n  }\n  *{box-sizing:border-box;}\n  html{-webkit-text-size-adjust:100%;}\n  body{margin:0;background:#fff;color:var(--aobo-text);\n    font-family:-apple-system,BlinkMacSystemFont,\"Segoe UI\",Roboto,\"Helvetica Neue\",Arial,sans-serif;\n    font-size:15px;line-height:1.6;}\n\n  \/* Root scope \u2014 WordPress theme guard *\/\n  .ts-props{color:var(--aobo-text);background:transparent;padding:0;box-sizing:border-box;line-height:1.6;}\n  .ts-props *{box-sizing:border-box;}\n  .ts-props button,.ts-props input[type=\"text\"]{\n    background:none !important;border:none !important;border-radius:0 !important;padding:0 !important;\n    margin:0 !important;font-size:inherit !important;font-weight:inherit !important;\n    letter-spacing:normal !important;text-transform:none !important;box-shadow:none !important;\n    line-height:inherit !important;text-decoration:none !important;}\n\n  .aobo-wrap{max-width:1160px;margin:0 auto;}\n\n  \/* Hero *\/\n  .ts-hero{background:#fff;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);overflow:hidden;}\n  .ts-hero-top{padding:1.5em;background:var(--aobo-stripe);border-bottom:1px solid var(--aobo-border);}\n  .ts-kicker{display:inline-flex;align-items:center;gap:6px;color:var(--aobo-accent);background:var(--aobo-hover);\n    border:1px solid var(--aobo-border);border-radius:var(--aobo-radius-sm);padding:4px 8px;\n    font-size:.85em;font-weight:600;margin-bottom:.8em;}\n  .ts-kicker span{width:6px;height:6px;background:var(--aobo-orange);border-radius:50%;display:inline-block;}\n  .ts-hero h1{margin:0;font-size:2rem;line-height:1.3;color:var(--aobo-text);text-align:center;}\n  .ts-hero-top p{margin:.6em auto 0;max-width:820px;font-size:.9em;line-height:1.6;color:var(--aobo-muted);text-align:center;}\n\n  \/* Tool area *\/\n  .ts-tool-area{padding:1.5em;}\n\n  \/* Legend *\/\n  .ts-legend{display:flex;flex-wrap:wrap;gap:8px;margin-bottom:1em;}\n  .ts-legend > span{display:inline-flex;align-items:center;gap:5px;font-size:.8em;color:var(--aobo-muted);\n    background:var(--aobo-stripe);border:1px solid var(--aobo-border);border-radius:var(--aobo-radius-sm);\n    padding:3px 8px;}\n  .ts-legend b{color:var(--aobo-text);font-weight:600;}\n  .ts-legend .ts-dot{width:9px;height:9px;border-radius:50%;background:var(--aobo-accent);display:inline-block;\n    padding:0;border:0;gap:0;}\n\n  \/* Controls *\/\n  .ts-controls{display:flex;flex-wrap:wrap;gap:10px;align-items:center;background:var(--aobo-stripe);\n    border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);padding:1em;margin-bottom:1.2em;}\n  .ts-search{flex:1 1 220px;max-width:340px;position:relative;}\n  .ts-props .ts-search input{width:100% !important;border:1px solid var(--aobo-border-dark) !important;\n    border-radius:var(--aobo-radius-sm) !important;padding:.5em .6em .5em 2em !important;\n    font-size:.92em !important;color:var(--aobo-text) !important;background:#fff !important;\n    outline:none !important;box-shadow:none !important;}\n  .ts-props .ts-search input:focus{border-color:var(--aobo-accent) !important;\n    box-shadow:0 0 0 2px rgba(37,99,235,.12) !important;}\n  .ts-search::before{content:\"\";position:absolute;left:.7em;top:50%;transform:translateY(-50%);\n    width:13px;height:13px;background:var(--aobo-muted);\n    -webkit-mask:url(\"data:image\/svg+xml;utf8,<svg xmlns='http:\/\/www.w3.org\/2000\/svg' viewBox='0 0 24 24' fill='none' stroke='black' stroke-width='2'><circle cx='11' cy='11' r='8'\/><path d='m21 21-4.3-4.3'\/><\/svg>\") center\/contain no-repeat;\n    mask:url(\"data:image\/svg+xml;utf8,<svg xmlns='http:\/\/www.w3.org\/2000\/svg' viewBox='0 0 24 24' fill='none' stroke='black' stroke-width='2'><circle cx='11' cy='11' r='8'\/><path d='m21 21-4.3-4.3'\/><\/svg>\") center\/contain no-repeat;}\n  .ts-chips{display:flex;flex-wrap:wrap;gap:6px;}\n  .ts-props .ts-chip{border:1px solid var(--aobo-border-dark) !important;background:#fff !important;\n    color:var(--aobo-text) !important;border-radius:999px !important;padding:.4em .9em !important;\n    font-size:.8em !important;font-weight:600 !important;cursor:pointer !important;transition:all .15s !important;}\n  .ts-props .ts-chip:hover{background:var(--aobo-hover) !important;border-color:var(--aobo-accent) !important;}\n  .ts-props .ts-chip.on{background:var(--aobo-accent) !important;border-color:var(--aobo-accent) !important;color:#fff !important;}\n  .ts-count{font-size:.8em;color:var(--aobo-muted);margin-left:auto;white-space:nowrap;}\n\n  \/* Table *\/\n  .ts-table-wrap{overflow-x:auto;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);\n    background:#fff;box-shadow:0 1px 2px rgba(16,24,40,.04);}\n  table.ts-table{border-collapse:collapse;width:100%;min-width:880px;font-size:.88em;}\n  .ts-table thead th{position:sticky;top:0;z-index:2;background:var(--aobo-accent-dark);color:#fff;\n    border-bottom:0;border-right:1px solid rgba(255,255,255,.1);text-align:center;padding:.6em .7em;\n    font-size:.82em;font-weight:600;text-transform:none;letter-spacing:.02em;cursor:pointer;\n    white-space:nowrap;user-select:none;}\n  .ts-table thead th:last-child{border-right:0;}\n  .ts-table thead th .ts-arr{color:#ffd166;font-weight:700;margin-left:3px;}\n  .ts-table tbody td{padding:.55em .7em;border-bottom:1px solid var(--aobo-border);text-align:center;\n    vertical-align:middle;white-space:nowrap;}\n  .ts-table tbody tr:nth-child(even){background:var(--aobo-stripe);}\n  .ts-table tbody tr:hover{background:var(--aobo-hover);}\n  .ts-table tbody tr.ts-group td{background:#e8ecf1;font-weight:700;font-size:.78em;letter-spacing:.05em;\n    text-transform:uppercase;color:#3c4043;padding:.55em .7em;border-bottom:1px solid var(--aobo-border);\n    text-align:left;}\n  .ts-table tbody tr:not(.ts-group).ts-hide{display:none;}\n  td.ts-grade{font-weight:700;font-size:.95em;text-align:left;white-space:nowrap;color:var(--aobo-text);}\n  .ts-meter{display:inline-flex;align-items:center;gap:7px;}\n  .ts-meter i{display:inline-block;width:44px;height:6px;border-radius:3px;background:var(--aobo-fill);overflow:hidden;}\n  .ts-meter i b{display:block;height:100%;border-radius:3px;background:linear-gradient(90deg,#4d94ff,var(--aobo-accent));}\n  .ts-meter span{font-size:.9em;font-weight:600;min-width:14px;}\n  .ts-hr{font-variant-numeric:tabular-nums;font-weight:500;}\n  .ts-num{font-variant-numeric:tabular-nums;}\n  .ts-sup{font-size:9px;color:var(--aobo-accent);vertical-align:super;line-height:0;}\n\n  \/* Footnotes *\/\n  .ts-notes-list{margin:1.2em 0 0;background:#fff;border:1px solid var(--aobo-border);\n    border-left:3px solid var(--aobo-accent);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;\n    padding:1em 1.2em 1em 2.2em;font-size:.82em;color:var(--aobo-muted);line-height:1.7;}\n  .ts-notes-list li{margin-bottom:.3em;}\n  .ts-notes-list sup{color:var(--aobo-accent);font-size:10px;}\n\n  \/* Figure *\/\n  .ts-fig{margin:1.2em 0 0;background:#fff;border:1px solid var(--aobo-border);border-radius:var(--aobo-radius);padding:1em;}\n  .ts-fig img{display:block;width:100%;height:auto;border-radius:6px;}\n  .ts-fig figcaption{font-size:.8em;color:var(--aobo-muted);margin-top:.6em;line-height:1.6;}\n  .ts-fig figcaption b{color:var(--aobo-text);}\n\n  \/* Info cards *\/\n  .ts-grid{display:grid;grid-template-columns:repeat(auto-fit,minmax(250px,1fr));gap:14px;margin-top:1.2em;}\n  .ts-grid .ts-card{background:#fff;border:1px solid var(--aobo-border);border-left:3px solid var(--aobo-accent);\n    border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;padding:1em 1.2em;}\n  .ts-grid h2{font-size:1em;margin:0 0 .4em;color:var(--aobo-text);}\n  .ts-grid p{font-size:.82em;color:var(--aobo-muted);margin:0;line-height:1.7;}\n  .ts-grid p b{color:var(--aobo-text);font-weight:600;}\n\n  \/* Disclaimer *\/\n  .ts-disclaimer{margin-top:1.2em;background:#fff;border:1px solid var(--aobo-border);\n    border-left:3px solid var(--aobo-accent);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;\n    padding:1em 1.2em;}\n  .ts-disclaimer h3{margin:0 0 .5em;font-size:.95em;color:var(--aobo-text);display:flex;align-items:center;gap:6px;}\n  .ts-disclaimer h3::before{content:\"\\2139\";font-size:1em;color:var(--aobo-accent);}\n  .ts-disclaimer p{margin:0 0 .5em;max-width:none;color:var(--aobo-muted);line-height:1.7;}\n  .ts-disclaimer p:last-child{margin-bottom:0;}\n\n  \/* Empty \/ source *\/\n  .ts-empty{display:none;text-align:center;color:var(--aobo-muted);padding:2em 1em;font-size:.9em;}\n  .ts-empty.show{display:block;}\n  .ts-source{margin-top:.8em;color:var(--aobo-muted);font-size:.82em;line-height:1.58;}\n\n  @media (max-width:860px){\n    .ts-hero-top,.ts-tool-area{padding:1em;}\n    .ts-controls{flex-direction:column;align-items:stretch;}\n    .ts-search{max-width:none;}\n    .ts-count{margin-left:0;}\n    .ts-hero h1{font-size:1.5rem;}\n  }\n  @media (max-width:520px){\n    .ts-hero-top,.ts-tool-area{padding:.8em;}\n    table.ts-table{font-size:.82em;}\n    .ts-table thead th,.ts-table tbody td{padding:.4em .4em;}\n  }\n  table.ts-table thead th{cursor:default;}\n  table.ts-table td.ts-grade{font-weight:700;}\n  table.ts-table td.ts-type{white-space:normal;text-align:left;font-size:.92em;color:#555;min-width:150px;}\n  table.ts-table td.ts-long{white-space:normal;text-align:left;vertical-align:top;font-size:.92em;color:#444;\n    min-width:260px;line-height:1.55;}\n  table.ts-table td.ts-safe{white-space:normal;text-align:left;vertical-align:top;}\n  table.ts-table tbody tr:hover{background:var(--aobo-hover);}\n  table.ts-table tbody tr.ts-group:hover td{background:#e8ecf1;}\n  .ts-sec{margin:1.8em 0 .5em;font-size:1.02em;color:var(--aobo-text);font-weight:700;}\n  .ts-sec span{display:block;font-size:.8em;font-weight:400;color:var(--aobo-muted);margin-top:.15em;line-height:1.6;}\n  .ts-table-wrap{margin-top:.6em;}\n  .ts-tcap{margin:.5em 0 0;font-size:.78em;color:var(--aobo-muted);line-height:1.6;}\n  .ts-props a{color:var(--aobo-blue) !important;text-decoration:none !important;}\n  .ts-props a:hover{text-decoration:underline !important;}\n  .ts-rel{margin-top:1.2em;background:#fff;border:1px solid var(--aobo-border);\n    border-left:3px solid var(--aobo-blue);border-radius:0 var(--aobo-radius) var(--aobo-radius) 0;padding:1em 1.2em;}\n  .ts-rel h3{margin:0 0 .5em;font-size:.95em;color:var(--aobo-text);}\n  .ts-rel p{margin:0;font-size:.85em;line-height:1.9;color:var(--aobo-muted);}\n  .ts-rel p a{font-weight:600;}\n\n  .aobo-ht-ref.ts-props table.ts-table.wraphead thead th{white-space:normal;line-height:1.25;}\n  .aobo-ht-ref.ts-props table.ts-table.wraphead tbody td{white-space:nowrap !important;}\n<\/style>\n\n<style id=\"aobo-dl-css\">\n.aobo-ht-ref.ts-props .ts-dl{display:flex !important;flex-wrap:wrap;align-items:center;gap:1em;\n  background:var(--aobo-stripe) !important;border:1px solid var(--aobo-border) !important;\n  border-radius:var(--aobo-radius) !important;padding:1.1em 1.3em !important;margin:1.5em 0 !important;}\n.aobo-ht-ref.ts-props .ts-dl-txt{flex:1 1 340px;font-size:.95em;color:var(--aobo-text) !important;line-height:1.55;}\n.aobo-ht-ref.ts-props .ts-dl-txt strong{display:block;font-weight:700 !important;margin-bottom:.2em;color:var(--aobo-text) !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn{display:inline-flex !important;align-items:center;gap:.5em;\n  background:var(--aobo-blue) !important;color:#fff !important;border:1px solid var(--aobo-blue) !important;\n  border-radius:var(--aobo-radius-sm) !important;padding:.75em 1.35em !important;font-size:.95em !important;\n  font-weight:600 !important;text-decoration:none !important;white-space:nowrap;box-shadow:none !important;\n  line-height:1.3 !important;text-transform:none !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn:hover,.aobo-ht-ref.ts-props a.ts-dl-btn:focus{background:var(--aobo-blue-dark) !important;\n  border-color:var(--aobo-blue-dark) !important;color:#fff !important;}\n.aobo-ht-ref.ts-props a.ts-dl-btn svg{width:1.05em;height:1.05em;fill:none;stroke:currentColor;stroke-width:2;flex:0 0 auto;}\n@media (max-width:640px){.aobo-ht-ref.ts-props a.ts-dl-btn{width:100%;justify-content:center;}}\n<\/style>\n\n<style id=\"aobo-ds\">\n.entry-content[class]{--ds-font-body: Lora,serif;--ds-font-head: Lato,sans-serif;--ds-blue: #0c56d0;--ds-blue-deep: #082d6f;--ds-blue-dark: #073b91;--ds-blue-soft: #eaf2ff;--ds-blue-pale: #f7fbff;--ds-border: #d7e5fb;--ds-border-soft: #e8eef8;--ds-text: #203044;--ds-muted: #617087;--ds-orange: #f59b23;--ds-shadow: 0 18px 45px rgba(12,86,208,0.10);--ds-shadow-sm: 0 12px 32px rgba(12,86,208,0.07);font-family: var(--ds-font-body);line-height: 1.7;-webkit-text-size-adjust: 100%;box-sizing: border-box}.entry-content[class] *,.entry-content[class] *::before,.entry-content[class] *::after{box-sizing: border-box}.entry-content[class] h1{font-family: var(--ds-font-head) !important;font-size: clamp(24px,4vw,min(50px,var(--h1-max,50px))) !important;line-height: 1.08 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 0 0 16px !important}.entry-content[class] h2{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 44px 0 16px !important}.entry-content[class] h3{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.3 !important;letter-spacing: 0 !important;font-weight: 400 !important;margin: 30px 0 12px !important}.entry-content[class] h4{font-family: var(--ds-font-head) !important;font-size: 19px !important;line-height: 1.35 !important;letter-spacing: 0 !important;font-weight: 700 !important;margin: 24px 0 10px !important}.entry-content[class] p,.entry-content[class] li,.entry-content[class] dd,.entry-content[class] dt{font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important}.entry-content[class] figcaption,.entry-content[class] small,.entry-content[class] .aobo-figure figcaption{font-size: 15px !important;line-height: 1.6 !important}.entry-content[class] table{width: 100%;border-collapse: collapse;background: #ffffff}.entry-content[class] table th,.entry-content[class] table thead th,.entry-content[class] table thead td{background: var(--ds-blue-soft) !important;color: var(--ds-blue-deep) !important;font-family: var(--ds-font-head) !important;font-size: 15px !important;font-weight: 700 !important;line-height: 1.45 !important;text-align: center !important;text-transform: none !important;letter-spacing: 0 !important;padding: 14px 16px !important;border: 0 !important;border-bottom: 1px solid var(--ds-border) !important;vertical-align: top !important;position: static !important}.entry-content[class] table td{font-family: var(--ds-font-body) !important;font-size: 15px !important;line-height: 1.55 !important;padding: 14px 16px !important;border: 0;border-bottom: 1px solid var(--ds-border-soft) !important;vertical-align: top !important;white-space: normal !important;text-align: center !important}.entry-content[class] table tbody tr:last-child td{border-bottom: 0 !important}.entry-content[class] table th.ds-text,.entry-content[class] table td.ds-text{text-align: left !important}.entry-content[class] table tbody tr:nth-child(even){background: #fafcff !important}.entry-content[class] table tbody tr:hover{background: #f2f7ff !important}.entry-content[class] table tbody td:first-child{color: var(--ds-blue-deep);font-weight: 700}.entry-content[class] .aobo-table-wrap,.entry-content[class] .ts-table-wrap{overflow-x: auto;margin: 22px 0 28px;border: 1px solid var(--ds-border);border-radius: 18px;box-shadow: var(--ds-shadow-sm);background: #ffffff}.entry-content[class] h1,.entry-content[class] h2,.entry-content[class] h3,.entry-content[class] h4{color: var(--ds-blue-deep)}.entry-content[class] p,.entry-content[class] li{color: var(--ds-text)}.entry-content[class] a{color: var(--ds-blue);font-weight: 700;text-decoration: none}.entry-content[class] a:hover,.entry-content[class] a:focus{color: var(--ds-orange)}.entry-content[class] .aobo-final-cta h1,.entry-content[class] .aobo-final-cta h2,.entry-content[class] .aobo-final-cta h3,.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-cta h1,.entry-content[class] .aobo-cta h2,.entry-content[class] .aobo-cta h3,.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-cta-buttons,.entry-content[class] .aobo-cta-buttons *,.entry-content[class] .aobo-esr .stat-band h2,.entry-content[class] .aobo-esr .stat-band h3,.entry-content[class] .aobo-esr .stat-band p,.entry-content[class] .aobo-esr .closing h2,.entry-content[class] .aobo-esr .closing h3,.entry-content[class] .aobo-esr .closing p,.entry-content[class] .footcta h2,.entry-content[class] .footcta h3,.entry-content[class] .footcta p,.entry-content[class] .bg-dark h2,.entry-content[class] .bg-dark h3,.entry-content[class] .bg-dark p,.entry-content[class] .ht-header h2,.entry-content[class] .ht-header h3,.entry-content[class] .ts-cta h2,.entry-content[class] .ts-cta h3,.entry-content[class] .aobo-sup .stats h2,.entry-content[class] .aobo-sup .stats h3,.entry-content[class] .aobo-sup .stats p,.entry-content[class] .aobo-sup .cta h2,.entry-content[class] .aobo-sup .cta h3,.entry-content[class] .aobo-sup .cta p{color: inherit}.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-sup .cta p{color: rgba(255,255,255,0.92)}.entry-content[class] .has-ast-global-color-0-background-color,.entry-content[class] .has-ast-global-color-0-background-color *,.entry-content[class] .contact-container,.entry-content[class] .contact-container *{color: #ffffff !important}.entry-content[class] .has-ast-global-color-0-background-color .label-text,.entry-content[class] .has-ast-global-color-0-background-color .label-text *,.entry-content[class] .contact-container .label-text{color: rgba(255,255,255,0.72) !important}.entry-content[class] .aobo-cta h1,.entry-content[class] .aobo-cta h2,.entry-content[class] .aobo-cta h3,.entry-content[class] .aobo-cta h4,.entry-content[class] .cta h1,.entry-content[class] .cta h2,.entry-content[class] .cta h3,.entry-content[class] .cta h4,.entry-content[class] .aobo-final-cta h1,.entry-content[class] .aobo-final-cta h2,.entry-content[class] .aobo-final-cta h3,.entry-content[class] .aobo-final-cta h4{color: #ffffff !important}.entry-content[class] .aobo-cta p,.entry-content[class] .aobo-cta li,.entry-content[class] .cta p,.entry-content[class] .cta li,.entry-content[class] .aobo-final-cta p,.entry-content[class] .aobo-final-cta li{color: rgba(255,255,255,0.93) !important}.entry-content[class] .aobo-cta p a,.entry-content[class] .aobo-cta li a,.entry-content[class] .cta p a,.entry-content[class] .cta li a,.entry-content[class] .aobo-final-cta p a,.entry-content[class] .aobo-final-cta li a{color: #ffffff !important;text-decoration: underline}.entry-content[class] .aobo-btn-inquiry{color: #ffffff !important}.entry-content[class] .aobo-cta .aobo-btn-inquiry,.entry-content[class] .aobo-final-cta .aobo-btn-inquiry{color: var(--ds-blue) !important}.entry-content[class] .aobo-wrap,.entry-content[class] .aobo-article{max-width: 1180px;margin: 0 auto;padding: 0}.entry-content[class] img{max-width: 100%;height: auto}.entry-content[class] figure{margin: 26px auto 34px;max-width: 860px}.entry-content[class] figure img{display: block;width: 100%;border: 1px solid var(--ds-border);border-radius: 18px;box-shadow: var(--ds-shadow-sm);background: #ffffff}.entry-content[class] .aobo-hero{background: linear-gradient(135deg,#ffffff 0%,#f7fbff 56%,#eaf2ff 100%);border: 1px solid var(--ds-border);border-radius: 28px;padding: 42px 38px;margin-bottom: 24px;box-shadow: var(--ds-shadow);overflow: hidden;position: relative}.entry-content[class] .aobo-hero::after{content: \"\";position: absolute;right: -90px;top: -90px;width: 260px;height: 260px;border-radius: 50%;background: rgba(12,86,208,0.08)}.entry-content[class] .aobo-hero h1,.entry-content[class] .aobo-hero p{position: relative;z-index: 2}.entry-content[class] .aobo-note-box{margin: 34px 0;padding: 22px 24px;border: 1px solid var(--ds-border);border-left: 5px solid var(--ds-orange);border-radius: 16px;background: #fbfdff}.entry-content[class] .aobo-note-box p{margin: 0 0 14px;color: var(--ds-muted) !important;font-style: italic}.entry-content[class] .aobo-note-box p:last-child{margin-bottom: 0}.entry-content[class] .aobo-btn{display: inline-flex;align-items: center;justify-content: center;min-height: 42px;padding: 10px 16px;border-radius: 999px;text-align: center;text-decoration: none;font-family: var(--ds-font-head) !important;font-weight: 700;font-size: 14px !important;line-height: 1.2;transition: all 0.2s ease;cursor: pointer;white-space: nowrap}.entry-content[class] .aobo-btn-primary{background: var(--ds-blue);border: 1px solid var(--ds-blue);color: #ffffff !important}.entry-content[class] .aobo-btn-secondary{background: #ffffff;border: 1px solid var(--ds-border);color: var(--ds-blue) !important}.entry-content[class] .aobo-btn:hover{transform: translateY(-1px)}.entry-content[class] .aobo-supply-actions{display: flex;flex-wrap: wrap;gap: 12px;margin-top: 18px}.entry-content[class] .aobo-supply-actions .aobo-btn{min-width: 190px}.entry-content[class] .aobo-final-cta{margin-top: 34px;padding: 34px;border-radius: 28px;background: linear-gradient(135deg,#073b91 0%,#0c56d0 100%);box-shadow: 0 18px 45px rgba(12,86,208,0.20);display: flex;align-items: center;justify-content: space-between;gap: 20px;flex-wrap: wrap}.entry-content[class] .aobo-final-cta h2{margin: 0 0 12px !important;font-size: 26px !important;color: #ffffff !important}.entry-content[class] .aobo-final-cta p{margin: 0}.entry-content[class] .aobo-final-cta .aobo-btn-primary{background: #ffffff;border-color: #ffffff;color: var(--ds-blue) !important}.entry-content[class] .aobo-final-cta .aobo-btn-secondary{background: transparent;border-color: rgba(255,255,255,0.75);color: #ffffff !important}.entry-content[class] .ts-hero{background: transparent !important;border: 0 !important;border-radius: 0 !important;box-shadow: none !important}.entry-content[class] .ts-hero-top{background: linear-gradient(135deg,#ffffff 0%,#f7fbff 56%,#eaf2ff 100%) !important;border: 1px solid var(--ds-border) !important;border-radius: 28px !important;padding: 42px 38px !important;margin: 0 0 24px !important;box-shadow: var(--ds-shadow) !important;position: relative;overflow: hidden;text-align: left !important}.entry-content[class] .ts-hero-top h1,.entry-content[class] .ts-hero-top p,.entry-content[class] .ts-hero h1{text-align: left !important}.entry-content[class] .ts-hero-top p{max-width: none !important;margin: 0 0 12px !important}.entry-content[class] .ts-tool-area{padding: 0 !important}.entry-content[class] .ts-sec{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 44px 0 16px !important}.entry-content[class] .ts-sec > span{display: block !important;font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important;font-weight: 400 !important;color: var(--ds-text) !important;margin: 0 0 16px !important}.entry-content[class] .ts-kicker{display: inline-flex !important;align-items: center;gap: 7px;margin: 0 0 14px !important;padding: 6px 14px !important;border: 1px solid var(--ds-border) !important;border-radius: 999px !important;background: #ffffff !important;color: var(--ds-blue) !important;font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important;letter-spacing: 0 !important;text-transform: none !important}.entry-content[class] .ts-p,.entry-content[class] .card-desc,.entry-content[class] .aobo-strip-intro,.entry-content[class] .schema-faq-answer{font-family: var(--ds-font-body) !important;font-size: 17px !important;line-height: 1.7 !important;font-weight: 400 !important}.entry-content[class] .lead,.entry-content[class] .fund-lead{font-family: var(--ds-font-body) !important;font-size: 19px !important;line-height: 1.65 !important;font-weight: 400 !important}.entry-content[class] .ts-h2{font-family: var(--ds-font-head) !important;font-size: 30px !important;line-height: 1.25 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 44px 0 16px !important}.entry-content[class] .ts-h3{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.3 !important;font-weight: 400 !important;color: var(--ds-blue-deep) !important;margin: 30px 0 12px !important}.entry-content[class] .card-grade{font-family: var(--ds-font-head) !important;font-size: 23px !important;line-height: 1.25 !important;font-weight: 700 !important}.entry-content[class] .schema-faq-question{font-family: var(--ds-font-head) !important;font-size: 19px !important;line-height: 1.4 !important;font-weight: 700 !important;color: var(--ds-blue-deep) !important}.entry-content[class] .ts-source,.entry-content[class] .ts-hint,.entry-content[class] .ts-placeholder,.entry-content[class] .ht-spec-label,.entry-content[class] .ht-spec-value,.entry-content[class] .ht-step-indicator,.entry-content[class] .ht-badge,.entry-content[class] .idx,.entry-content[class] .xlink,.entry-content[class] .cat-note,.entry-content[class] .aobo-card-note,.entry-content[class] .card-desig,.entry-content[class] .k,.entry-content[class] .v,.entry-content[class] .note,.entry-content[class] .aobo-note{font-family: var(--ds-font-head) !important;font-size: 15px !important;line-height: 1.6 !important;font-weight: 400 !important}.entry-content[class] .ht-spec-label,.entry-content[class] .idx,.entry-content[class] .k{font-weight: 700 !important}.entry-content[class] .aobo-note,.entry-content[class] .note{font-family: var(--ds-font-body) !important;color: var(--ds-muted) !important}.entry-content[class] .chip{font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important}.entry-content[class] .kicker,.entry-content[class] .eyebrow,.entry-content[class] .aobo-eyebrow{display: inline-flex !important;align-items: center;gap: 7px;margin: 0 0 14px !important;padding: 6px 14px !important;border: 1px solid var(--ds-border) !important;border-radius: 999px !important;background: #ffffff !important;color: var(--ds-blue) !important;font-family: var(--ds-font-head) !important;font-size: 13px !important;font-weight: 700 !important;letter-spacing: 0 !important;text-transform: none !important}@media (max-width: 760px){.entry-content[class] h1{font-size: clamp(22px,6.4vw,min(34px,var(--h1-max,34px))) !important}.entry-content[class] h2{font-size: 25px !important}.entry-content[class] h3{font-size: 20px !important}.entry-content[class] h4{font-size: 17px !important}.entry-content[class] p,.entry-content[class] li{font-size: 16px !important}.entry-content[class] table th,.entry-content[class] table td{font-size: 14px !important;padding: 11px 12px !important}.entry-content[class] .aobo-hero{padding: 30px 22px}.entry-content[class] .aobo-final-cta{padding: 26px 22px}.entry-content[class] .aobo-final-cta .aobo-btn{width: 100%}}\n<\/style>\n<section class=\"aobo-ht-ref ts-props\">\n<div class=\"aobo-wrap\">\n\n<div class=\"ts-hero\">\n<div class=\"ts-hero-top\">\n<div class=\"ts-kicker\"><span><\/span>Tool Steel | Welding | Filler Metal Selection<\/div>\n<h1 style=\"--h1-max:46px\">Tool Steel Weld Filler Metals<\/h1>\n<p>A tool steel repair seldom runs on a standard covered electrode. The deposits that match a tool steel in service are proprietary products, and the choice between one of those, a carbon or low-alloy steel wire and a nonhardenable austenitic wire is set by where the deposit sits on the tool and what the tool has to do afterwards. This page sets out the three filler metal categories, the four selection factors, and the weld deposit compositions that are used across the tool steel groups.<\/p>\n<\/div>\n<\/div>\n\n<div class=\"ts-tool-area\">\n\n<h2 class=\"ts-h2\">Four factors decide the filler metal<\/h2>\n<p class=\"ts-p\">A filler metal for a tool or die is selected against four things. They are the composition of the base metal, the heat treated condition of the base metal, whether that is annealed or hardened and tempered, the service requirements of the weld deposit, and the post-weld heat treatment the part will receive. The heat treated condition carries as much weight as the composition, because the same grade welded annealed and welded at 52 HRC are two different jobs.<\/p>\n\n<h2 class=\"ts-h2\">The three categories of filler metal<\/h2>\n<p class=\"ts-p\">The first category produces weld deposits that correspond in hardenability or in composition to the basic tool steel types, the water hardening, oil hardening and air hardening cold work grades, the hot work grades and the high speed grades. These deposits come hard in the as-welded condition, and they are not covered by the standard filler metal specifications, which is why they are bought as proprietary products under a producer name rather than under an AWS classification. The table below gives the nominal composition of the deposits in this category.<\/p>\n<div class=\"ts-table-wrap\">\n<table class=\"ts-table\" style=\"min-width:900px;\">\n<thead><tr><th>AISI steel type<\/th><th>Filler-metal type<\/th><th>C<\/th><th>Mn<\/th><th>Si<\/th><th>Cr<\/th><th>Ni<\/th><th>V<\/th><th>W<\/th><th>Mo<\/th><\/tr><\/thead>\n<tbody>\n<tr><td>W1, W2<\/td><td class=\"ts-type\">Water-hardening<\/td><td class=\"ts-num\">0.95<\/td><td class=\"ts-num\">0.30<\/td><td class=\"ts-num\">0.20<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">0.20<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">. . .<\/td><\/tr>\n<tr><td>S1, S5, S7<\/td><td class=\"ts-type\">Hot-work<\/td><td class=\"ts-num\">0.33<\/td><td class=\"ts-num\">0.40<\/td><td class=\"ts-num\">1.00<\/td><td class=\"ts-num\">5.00<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">1.25<\/td><td class=\"ts-num\">1.35<\/td><\/tr>\n<tr><td>O1, O6<\/td><td class=\"ts-type\">Oil-hardening<\/td><td class=\"ts-num\">0.92<\/td><td class=\"ts-num\">1.28<\/td><td class=\"ts-num\">0.30<\/td><td class=\"ts-num\">0.50<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">0.50<\/td><td class=\"ts-num\">. . .<\/td><\/tr>\n<tr><td>A2, A4, D2<\/td><td class=\"ts-type\">Air-hardening<\/td><td class=\"ts-num\">0.95<\/td><td class=\"ts-num\">0.40<\/td><td class=\"ts-num\">0.30<\/td><td class=\"ts-num\">5.25<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">0.25<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">1.10<\/td><\/tr>\n<tr><td>H11, H12, H13<\/td><td class=\"ts-type\">Hot-work<\/td><td class=\"ts-num\">0.33<\/td><td class=\"ts-num\">0.40<\/td><td class=\"ts-num\">1.00<\/td><td class=\"ts-num\">5.00<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">1.25<\/td><td class=\"ts-num\">1.35<\/td><\/tr>\n<tr><td>M1, M2, M10, T1, T2, T4<\/td><td class=\"ts-type\">High-speed<\/td><td class=\"ts-num\">0.90<\/td><td class=\"ts-num\">0.30<\/td><td class=\"ts-num\">0.35<\/td><td class=\"ts-num\">4.00<\/td><td class=\"ts-num\">. . .<\/td><td class=\"ts-num\">1.00<\/td><td class=\"ts-num\">1.50<\/td><td class=\"ts-num\">8.00<\/td><\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p class=\"ts-tcap\"><em>Source, Table 19 of Welding of Low-Alloy Steels, in ASM Handbook Volume 6, Welding, Brazing and Soldering. Compositions of similar types of weld metal from different producers can vary.<\/em><\/p>\n<p class=\"ts-p\">Composition data is for general reference only. Actual values vary by standard, mill, and heat number. Confirm against the material test certificate (MTC) or contact Aobo Steel.<\/p>\n<p class=\"ts-p\">The second category runs the other way on matching. It covers carbon and low-alloy steel deposits with moderate hardness and toughness as welded or stress relieved. Some of them respond to a quench and temper cycle, and most are intended for work where the deposit does not have to match the hardened tool steel. These grades sit inside the ANSI and AWS specifications for carbon steel and low-alloy steel filler metals, so they are stocked rather than made to order.<\/p>\n<p class=\"ts-p\">The third category is nonhardenable. Austenitic stainless steels, the nickel-chromium-iron, nickel-copper and copper-nickel alloys all fall here. Their value is ductility. When a tool that is already hardened has to be repaired, a ductile deposit resists both weld metal cracking and base metal cracking far better than a hard deposit does, and the same wires are useful for building up worn tooling before a hard surface is put on top. A nonhardenable deposit can be overlaid with a hardfacing deposit to restore a hard, wear resistant surface over it.<\/p>\n\n<h2 class=\"ts-h2\">Matching hardenability rather than matching composition<\/h2>\n<p class=\"ts-p\">On many tool steel welds the requirement is that the weld metal and the base metal respond to heat treatment in a similar way, so that the weld metal finishes at the same hardness as the base metal after a quench and temper. That usually means matching the composition of the base metal, and it does not have to. A deposit carrying less carbon and more alloy can reach the same final hardness or strength, and dropping the carbon in the weld metal generally lowers the risk of weld cracking and improves the toughness of the deposit. Where the goal is a hard, wear resistant deposit that survives, the carbon content of the deposit is the number to watch.<\/p>\n\n<h2 class=\"ts-h2\">Where the deposit sits sets how strict the match has to be<\/h2>\n<p class=\"ts-p\">A weld that lands in a functional area of the tool, on a cutting edge or a wear surface, has to be selected for hardness. The deposit must reach the hardness or strength the surface needs either as welded or after a stress relief or temper, without a separate hardening treatment, because a finished tool often cannot be quenched again without losing its dimensions. A weld that lands away from the working area is a different problem. There the deposit only has to hold the tool together, so it can be chosen for maximum crack resistance, ductility and toughness instead of for hardness. On a repair of a worn tool or a tool built up from components, that freedom is worth taking.<\/p>\n<p class=\"ts-p\">Where a soft deposit is used to fill volume under a hard one, the tool steel layer above it still has to be thick enough to absorb dilution from the layer underneath and to keep the wear properties it was chosen for. Dilution is the reason a shallow deposit rarely performs the way the filler metal data sheet suggests.<\/p>\n\n<p class=\"ts-source\">Source: ASM Handbook, Volume 6, Welding, Brazing and Soldering, ASM International, 1993.<\/p>\n\n<\/div><\/div><\/div><\/section>\n","protected":false},"excerpt":{"rendered":"<p>Tool Steel | Welding | Filler Metal Selection Tool Steel Weld Filler Metals A tool steel repair seldom runs on a standard covered electrode. The deposits that match a tool steel in service are proprietary products, and the choice between one of those, a carbon or low-alloy steel wire and a nonhardenable austenitic wire is [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-21119","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.6 (Yoast SEO v28.6) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Tool Steel Weld Filler Metals, Deposits for Each Tool Steel Group<\/title>\n<meta name=\"description\" content=\"The three filler metal categories used on tool and die steels, the weld deposit compositions matched to each tool steel group, and how to choose by repair location.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/tool-steel-weld-filler-metals\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Tool Steel Weld Filler Metals\" \/>\n<meta property=\"og:description\" content=\"The three filler metal categories used on tool and die steels, the weld deposit compositions matched to each tool steel group, and how to choose by repair location.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/tool-steel-weld-filler-metals\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"4 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-weld-filler-metals\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-weld-filler-metals\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Tool Steel Weld Filler Metals\",\"datePublished\":\"2026-10-07T08:10:25+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-weld-filler-metals\\\/\"},\"wordCount\":870,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-weld-filler-metals\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-weld-filler-metals\\\/\",\"name\":\"Tool Steel Weld Filler Metals, Deposits for Each Tool Steel Group\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-07T08:10:25+00:00\",\"description\":\"The three filler metal categories used on tool and die steels, the weld deposit compositions matched to each tool steel group, and how to choose by repair location.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-weld-filler-metals\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-weld-filler-metals\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-weld-filler-metals\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Tool Steel Weld Filler Metals\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Tool Steel Weld Filler Metals, Deposits for Each Tool Steel Group","description":"The three filler metal categories used on tool and die steels, the weld deposit compositions matched to each tool steel group, and how to choose by repair location.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/tool-steel-weld-filler-metals\/","og_locale":"pt_BR","og_type":"article","og_title":"Tool Steel Weld Filler Metals","og_description":"The three filler metal categories used on tool and die steels, the weld deposit compositions matched to each tool steel group, and how to choose by repair location.","og_url":"https:\/\/aobosteel.com\/pt\/tool-steel-weld-filler-metals\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"4 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-weld-filler-metals\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-weld-filler-metals\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Tool Steel Weld Filler Metals","datePublished":"2026-10-07T08:10:25+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-weld-filler-metals\/"},"wordCount":870,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-weld-filler-metals\/","url":"https:\/\/aobosteel.com\/tool-steel-weld-filler-metals\/","name":"Tool Steel Weld Filler Metals, Deposits for Each Tool Steel Group","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-07T08:10:25+00:00","description":"The three filler metal categories used on tool and die steels, the weld deposit compositions matched to each tool steel group, and how to choose by repair location.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-weld-filler-metals\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-weld-filler-metals\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-weld-filler-metals\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Tool Steel Weld Filler Metals"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Tool Steel | Welding | Filler Metal Selection Tool Steel Weld Filler Metals A tool steel repair seldom runs on a standard covered electrode. The deposits that match a tool steel in service are proprietary products, and the choice between one of those, a carbon or low-alloy steel wire and a nonhardenable austenitic wire is&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Tool Steel | Welding | Filler Metal Selection Tool Steel Weld Filler Metals A tool steel repair seldom runs on a standard covered electrode. The deposits that match a tool steel in service are proprietary products, and the choice between one of those, a carbon or low-alloy steel wire and a nonhardenable austenitic wire is&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21119","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=21119"}],"version-history":[{"count":1,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21119\/revisions"}],"predecessor-version":[{"id":21120,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/21119\/revisions\/21120"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=21119"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}