{"id":20798,"date":"2026-10-03T16:12:27","date_gmt":"2026-10-03T08:12:27","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20798"},"modified":"2026-10-16T01:13:45","modified_gmt":"2026-10-15T17:13:45","slug":"pm-tool-steel-properties","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/pm-tool-steel-properties\/","title":{"rendered":"Propriedades do a\u00e7o-ferramenta P\/M, tamanho de carboneto, desgaste e tenacidade"},"content":{"rendered":"<h1 class=\"wp-block-heading\">Propriedades do a\u00e7o-ferramenta P\/M, tamanho de carboneto, desgaste e tenacidade<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">O a\u00e7o-ferramenta de metalurgia do p\u00f3 \u00e9 comprado por um motivo. Os carbonetos nele s\u00e3o pequenos e distribu\u00eddos uniformemente, em vez de grosseiros e em bandas. Todo o resto sobre o grau decorre disso, e os gr\u00e1ficos desta p\u00e1gina medem isso. O carboneto prim\u00e1rio mediano no CPM T15 \u00e9 1,3 &#181;m contra 6,2 &#181;m no a\u00e7o convencional do mesmo grau, e o ensaio de desgaste que decorre disso coloca um grau P\/M ao van\u00e1dio uma ordem de magnitude \u00e0 frente de <a href=\"https:\/\/aobosteel.com\/pt\/d2-tool-steel\/\">D2<\/a>. Esta p\u00e1gina re\u00fane a distribui\u00e7\u00e3o do tamanho de carboneto, as microestruturas, os dados de desgaste de cilindros cruzados, os dados de impacto Charpy e as raz\u00f5es de retifica\u00e7\u00e3o para os a\u00e7os-ferramenta P\/M e seus equivalentes convencionais.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">O que a rota do p\u00f3 muda<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Um a\u00e7o-ferramenta convencional \u00e9 fundido e vazado, ent\u00e3o os carbonetos se formam durante a solidifica\u00e7\u00e3o e o \u00faltimo l\u00edquido a solidificar \u00e9 rico em carbono e liga. Isso produz bandas de carboneto e produz uma popula\u00e7\u00e3o de carbonetos com uma cauda longa de part\u00edculas grandes. Na rota P\/M, o banho \u00e9 atomizado a g\u00e1s em p\u00f3, cada part\u00edcula solidifica por conta pr\u00f3pria, e o p\u00f3 \u00e9 ent\u00e3o consolidado por prensagem isost\u00e1tica a quente, extrus\u00e3o ou forjamento. A segrega\u00e7\u00e3o de carboneto s\u00f3 pode acontecer dentro de uma part\u00edcula de algumas dezenas de microns, ent\u00e3o ap\u00f3s a consolida\u00e7\u00e3o a estrutura \u00e9 uniforme na escala da pe\u00e7a em vez da escala do lingote.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A medi\u00e7\u00e3o que diz tudo isso em uma linha \u00e9 a distribui\u00e7\u00e3o do tamanho de carboneto prim\u00e1rio abaixo. A curva do CPM T15 \u00e9 um pico estreito, mediana 1,3 &#181;m e m\u00e9dia 1,4 &#181;m. A curva do T15 convencional atinge o pico mais tarde e arrasta uma cauda at\u00e9 um m\u00e1ximo de 34 &#181;m. Um carboneto de 34 &#181;m \u00e9 um s\u00edtio de inicia\u00e7\u00e3o de trinca na aresta de uma ferramenta, e \u00e9 a part\u00edcula que lasca primeiro.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png\" alt=\"Primary carbide size distribution curves for CPM T15 and conventional T15 high speed steel\"\/><figcaption class=\"wp-element-caption\">Fig. 3. Distribui\u00e7\u00e3o do tamanho dos carbonetos prim\u00e1rios no a\u00e7o r\u00e1pido CPM T15 e no T15 convencional (fonte 1846). A curva do CPM \u00e9 um pico estreito, mediana 1,3 &#181;m e m\u00e9dia 1,4 &#181;m. A curva do convencional atinge o pico mais tarde e arrasta uma cauda at\u00e9 um m\u00e1ximo de 34 &#181;m, mediana 6,2 &#181;m e m\u00e9dia 9,5 &#181;m. Redesenhado a partir da figura da fonte, com ambas as curvas digitalizadas do gr\u00e1fico publicado.<\/figcaption><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">A rota do p\u00f3 n\u00e3o \u00e9 a \u00fanica forma de produzir um a\u00e7o r\u00e1pido, e as tr\u00eas rotas de produ\u00e7\u00e3o diferem em mais do que o tamanho do carboneto.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-totten-table-11-5-high-speed-steel-osprey-pm-ingot-properties.jpg\" alt=\"Comparison of properties of high speed tool steel made by the Osprey, powder metallurgy and ingot routes: carbide size, bend strength, wear resistance, grindability and toughness\"\/><figcaption class=\"wp-element-caption\">Tabela 11.5. Compara\u00e7\u00e3o de propriedades (valores relativos) do a\u00e7o r\u00e1pido para ferramentas produzido pelas rotas Osprey, metalurgia do p\u00f3 e metalurgia de lingote. O tamanho do carboneto \u00e9 dado em micr\u00f3metros e as outras quatro propriedades s\u00e3o valores relativos numa escala comum: resist\u00eancia \u00e0 flex\u00e3o, resist\u00eancia ao desgaste, retificabilidade e tenacidade. A rota do p\u00f3 apresenta o carboneto mais fino e a melhor combina\u00e7\u00e3o, a rota Osprey situa-se entre esta e a rota do lingote, e a rota do lingote tem o carboneto mais grosso e a menor tenacidade. Fonte: E. Essadiqi, Tool Steels, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Tabela 11.5.<\/figcaption><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">A estrutura que acompanha isso<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">As micrografias abaixo s\u00e3o os mesmos dois graus na mesma amplia\u00e7\u00e3o. No CPM T15 os carbonetos s\u00e3o um campo fino e uniforme; no T15 convencional s\u00e3o grosseiros e dispostos em bandas, que \u00e9 a estrutura deixada pela segrega\u00e7\u00e3o. A terceira figura faz a mesma compara\u00e7\u00e3o em um a\u00e7o para matriz em vez de uma ferramenta de corte, e separa as duas rotas convencionais da rota do p\u00f3. O H13 convencional padr\u00e3o \u00e9 grosseiro e fortemente bandado; o H13 convencional de qualidade premium, que \u00e9 feito com limites de segrega\u00e7\u00e3o mais apertados, \u00e9 mais fino mas ainda bandado; o H13 P\/M \u00e9 uniforme, sem bandas. O grau para trabalho a quente \u00e9 onde a diferen\u00e7a aparece como resist\u00eancia \u00e0 fadiga t\u00e9rmica em vez de lascamento de aresta, porque a trinca que come\u00e7a em uma banda de carboneto avan\u00e7a um pouco a cada ciclo.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-4-microstructure-t15.png\" alt=\"Micrograph comparison of CPM T15 and conventional T15 high speed steel\"\/><figcaption class=\"wp-element-caption\">Fig. 4. Microestruturas de a\u00e7o r\u00e1pido para ferramentas (fonte 1846). Esquerda, CPM T15; direita, T15 convencional. Os carbonetos no a\u00e7o convencional s\u00e3o grosseiros e bandeados, que \u00e9 o que a rota do p\u00f3 remove; os dois pain\u00e9is est\u00e3o na mesma amplia\u00e7\u00e3o. Reproduzido da figura da fonte (cortesia da Crucible Materials Corporation).<\/figcaption><\/figure>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-24-h13-microstructure.png\" alt=\"Longitudinal microstructure of standard conventional H13, premium quality conventional H13 and P\/M H13 die steel\"\/><figcaption class=\"wp-element-caption\">Fig. 24. Microestrutura longitudinal do H13 (fonte 1863), ataque de Vilella&#8217;s, 50&#215;. (a) H13 convencional padr\u00e3o, grosseiro e fortemente bandeado. (b) H13 convencional de qualidade premium, mais fino mas ainda bandeado. (c) H13 P\/M, uma popula\u00e7\u00e3o de carbonetos uniforme sem bandeamento. Reproduzido da figura da fonte.<\/figcaption><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">A vantagem que os n\u00fameros descrevem \u00e9 uma diferen\u00e7a na pr\u00f3pria estrutura, e \u00e9 vis\u00edvel numa \u00fanica amplia\u00e7\u00e3o.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-totten-fig-11-2-m3-high-speed-steel-pm-vs-ingot-microstructure.jpg\" alt=\"Microstructure of 100 mm diameter M3 high-speed steel bars, powder metallurgy against ingot casting, at the same magnification\"\/><figcaption class=\"wp-element-caption\">Fig. 11.2. Microestrutura de barras de 100 mm de di\u00e2metro de a\u00e7o r\u00e1pido M3 produzidas por (a) metalurgia do p\u00f3 e (b) fundi\u00e7\u00e3o em lingoteira, fotografadas na mesma amplia\u00e7\u00e3o. A barra P\/M apresenta uma popula\u00e7\u00e3o de carbonetos fina e uniformemente distribu\u00edda, enquanto a barra fundida em lingoteira mostra a rede de carbonetos grosseiros e o bandeamento deixado pela segrega\u00e7\u00e3o. Essa diferen\u00e7a no tamanho e na distribui\u00e7\u00e3o dos carbonetos \u00e9 o que os n\u00fameros de desgaste e tenacidade nesta p\u00e1gina est\u00e3o a medir. Fonte: E. Essadiqi, Tool Steels, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 11.2.<\/figcaption><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">Resist\u00eancia ao desgaste no ensaio de cilindros cruzados<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O ensaio de desgaste de cilindros cruzados pressiona dois cilindros um contra o outro sob carga e mede o volume perdido, e \u00e9 o ensaio que a ind\u00fastria de a\u00e7o-ferramenta cita para desgaste abrasivo. Leia os dois gr\u00e1ficos juntos. Os graus convencionais ficam na base da escala, H21 em 15, H19 em 25 e D2 em 30 no primeiro gr\u00e1fico, e D2 cerca de 15, O7 cerca de 25, A7 e M2 cerca de 30 no segundo. Os graus P\/M se separam deles por uma ordem de magnitude, e a separa\u00e7\u00e3o cresce com o teor de van\u00e1dio, CPM M4 em 150, CPM 9V em 150 e 270 em dois n\u00edveis de dureza, CPM T15 cerca de 400, e CPM 10V 515 em 60 HRC no primeiro gr\u00e1fico e cerca de 520 e 640 no segundo. O CPM 10V \u00e9 o grau para trabalho a frio de alto van\u00e1dio, e este ensaio \u00e9 a raz\u00e3o pela qual ele \u00e9 especificado para estampagem de longa produ\u00e7\u00e3o e para pe\u00e7as de desgaste que antes eram feitas em metal duro.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-19-wear-resistance-cpm-9v.png\" alt=\"Crossed cylinder wear test results for CPM 9V, CPM M4, CPM 10V, H21, H19 and D2 tool steel\"\/><figcaption class=\"wp-element-caption\">Fig. 19. Resultados do ensaio de desgaste de cilindros cruzados para o CPM 9V e outros a\u00e7os para ferramentas P\/M e convencionais na dureza indicada (fonte 1859). A fonte imprime os valores nas barras. H21 15 (57 HRC), H19 25 (56 HRC), D2 30 (62 HRC), CPM M4 150 (64 HRC), CPM 9V 150 (48 HRC), CPM 9V 270 (53 HRC), CPM 10V 515 (60 HRC), nas unidades que a fonte usa (10&#8311; MPa, com uma escala de 10&#185;&#8304; psi \u00e0 direita do original). Redesenhado a partir da figura da fonte, com os valores impressos retirados do gr\u00e1fico.<\/figcaption><\/figure>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-20-wear-resistance-cpm-10v.png\" alt=\"Crossed cylinder wear test results for CPM 10V, CPM M4, CPM T15, D2, O7, A7 and M2 tool steel\"\/><figcaption class=\"wp-element-caption\">Fig. 20. Resultados do ensaio de desgaste de cilindros cruzados para o CPM 10V e outros a\u00e7os para ferramentas P\/M e convencionais na dureza indicada (fonte 1860). A fonte n\u00e3o imprime nenhum valor nestas barras, portanto as leituras abaixo s\u00e3o retiradas do eixo e marcadas como aproximadas. D2 cerca de 15 (62 HRC), O7 cerca de 25 (61 HRC), A7 cerca de 30 (61 HRC), M2 cerca de 30 (64 HRC), CPM M4 cerca de 150 (64 HRC), CPM T15 cerca de 400 (67 HRC), CPM 10V cerca de 520 (60 HRC) e cerca de 640 (63 HRC). Redesenhado a partir da figura da fonte, com os valores lidos do gr\u00e1fico publicado (escala logar\u00edtmica).<\/figcaption><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">Tenacidade ao impacto nos mesmos graus<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Carbonetos finos ajudam a tenacidade assim como a resist\u00eancia ao desgaste, porque a part\u00edcula grosseira \u00e9 o que inicia a trinca. Nos dados de Charpy entalhe C abaixo, o CPM M4 atinge 46 J em 64 HRC enquanto o M4 convencional est\u00e1 em 16 J em 63 HRC, e o CPM 10V fica em 39 J em 60 HRC. A exce\u00e7\u00e3o vale a pena ler com aten\u00e7\u00e3o. O mesmo CPM 10V levado at\u00e9 63 HRC retorna 25 J, ent\u00e3o a vantagem de tenacidade \u00e9 trocada pela dureza no grau mais altamente ligado desta p\u00e1gina. Essa \u00e9 a troca normal, e \u00e9 por isso que os graus P\/M s\u00e3o encomendados na dureza que o trabalho precisa em vez da mais dura que o grau pode atingir.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-21-charpy-impact-cpm-10v.png\" alt=\"Charpy C notch impact energy for CPM 10V, CPM M4, M4, M2 and D2 tool steel\"\/><figcaption class=\"wp-element-caption\">Fig. 21. Propriedades de impacto Charpy entalhe C do CPM 10V e outros a\u00e7os para ferramentas P\/M e convencionais na dureza indicada (fonte 1860). A fonte imprime os valores nas barras. D2 25 J (62 HRC), M2 24 J (64 HRC), M4 16 J (63 HRC), CPM M4 46 J (64 HRC), CPM 10V 39 J (60 HRC) e CPM 10V 25 J (63 HRC). Redesenhado a partir da figura da fonte, com os valores impressos retirados do gr\u00e1fico.<\/figcaption><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">Retificabilidade<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00faltimo gr\u00e1fico \u00e9 o que decide o custo da oficina. A raz\u00e3o de retifica\u00e7\u00e3o \u00e9 o volume de metal removido dividido pelo volume de rebolo desgastado, ent\u00e3o um n\u00famero mais alto significa que o a\u00e7o retifica mais facilmente. Todo grau CPM supera seu equivalente convencional, M2S 16,1 contra 5,5, M3S-2 12,0 contra 2,2, M42 5,0 contra 1,8, T15 2,2 contra 0,6. Um a\u00e7o-ferramenta P\/M \u00e9 mais caro por quilograma e mais barato de acabar, e em uma ferramenta complexa o tempo de retifica\u00e7\u00e3o costuma ser o maior dos dois n\u00fameros.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-7-relative-grindability.png\" alt=\"Relative grindability bar chart for CPM and conventional high speed tool steels\"\/><figcaption class=\"wp-element-caption\">Fig. 7. Retificabilidade relativa dos a\u00e7os r\u00e1pidos para ferramentas CPM e convencionais (fonte 1850). A raz\u00e3o de retifica\u00e7\u00e3o \u00e9 o volume de metal removido dividido pelo volume de rebolo desgastado, portanto uma barra mais alta \u00e9 mais f\u00e1cil de retificar; a barra escura de cada par \u00e9 o grau CPM. CPM contra convencional, M2S 16,1 contra 5,5, M2 6,5 contra 3,9, M7 6,7 contra 2,4, M3S-2 12,0 contra 2,2, M42 5,0 contra 1,8, M4 2,7 contra 1,1, T15 2,2 contra 0,6. As tr\u00eas barras CPM isoladas s\u00e3o REX 20 em 3,5, REX 25 em 2,4 e REX 76 em 3,8. Redesenhado a partir da figura da fonte, com os valores impressos retirados do gr\u00e1fico.<\/figcaption><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">Quando especificar a rota do p\u00f3<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Os graus P\/M justificam seu pre\u00e7o onde o modo de falha est\u00e1 relacionado a carboneto, lascamento de aresta em uma ferramenta de alto van\u00e1dio, desgaste bandado em uma matriz de estampagem de longa produ\u00e7\u00e3o, trincamento por fadiga t\u00e9rmica em uma matriz para trabalho a quente, ou uma geometria de ferramenta que o rebolo precisa alcan\u00e7ar. Eles tamb\u00e9m s\u00e3o a resposta quando a alternativa \u00e9 o metal duro, j\u00e1 que um a\u00e7o para trabalho a frio P\/M oferece parte da resist\u00eancia ao desgaste do metal duro com a tenacidade e a usinabilidade do a\u00e7o-ferramenta. Para trabalho a frio comum em volume de produ\u00e7\u00e3o moderado, os convencionais <a href=\"https:\/\/aobosteel.com\/pt\/d2-tool-steel\/\">D2<\/a> e <a href=\"https:\/\/aobosteel.com\/pt\/m2-tool-steel\/\">M2<\/a> continuam sendo a escolha de valor, e o desgaste e a tenacidade que eles entregam s\u00e3o a linha de base contra a qual os gr\u00e1ficos acima s\u00e3o medidos. Os graus r\u00e1pidos P\/M e seus equivalentes convencionais s\u00e3o comparados por composi\u00e7\u00e3o na <a href=\"https:\/\/aobosteel.com\/pt\/pm-high-speed-steel-composition\/\">composi\u00e7\u00e3o do a\u00e7o r\u00e1pido PM<\/a> p\u00e1gina, a tenacidade das fam\u00edlias de a\u00e7o-ferramenta est\u00e1 reunida na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-impact-toughness-chart\/\">Tabela de tenacidade ao impacto do a\u00e7o ferramenta<\/a>, os dados de ensaio de desgaste abrasivo para os graus convencionais est\u00e3o na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-abrasive-wear-test-data\/\">Dados de ensaio de desgaste abrasivo de a\u00e7o para ferramentas<\/a> p\u00e1gina, a sele\u00e7\u00e3o de rebolo que acompanha as raz\u00f5es de retifica\u00e7\u00e3o est\u00e1 na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-grindability-and-grinding-wheel-selection\/\">Retificabilidade do A\u00e7o Ferramenta e Sele\u00e7\u00e3o de Rebolo<\/a> p\u00e1gina, e a se\u00e7\u00e3o que cada grau endurece est\u00e1 na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-hardenability-and-section-size\/\">T\u00eampera e Tamanho de Se\u00e7\u00e3o do A\u00e7o Ferramenta<\/a> p\u00e1gina.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Fonte: ASM Handbook, Vol 1, Properties and Selection: Irons, Steels and High-Performance Alloys.<\/p>","protected":false},"excerpt":{"rendered":"<p>P\/M Tool Steel Properties, Carbide Size, Wear and Toughness Powder metallurgy tool steel is bought for one reason. The carbides in it are small and evenly spread instead of coarse and banded. Everything else about the grade follows from that, and the charts on this page measure it. The median primary carbide in CPM T15 [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20798","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>P\/M Tool Steel Properties, Wear and Toughness<\/title>\n<meta name=\"description\" content=\"Carbide size, crossed-cylinder wear, Charpy impact and grinding ratios for P\/M and CPM tool steel against the conventional grades of the same type.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/pm-tool-steel-properties\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"P\/M Tool Steel Properties, Carbide Size, Wear and Toughness\" \/>\n<meta property=\"og:description\" content=\"Carbide size, crossed-cylinder wear, Charpy impact and grinding ratios for P\/M and CPM tool steel against the conventional grades of the same type.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/pm-tool-steel-properties\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T17:13:45+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"9 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"P\\\/M Tool Steel Properties, Carbide Size, Wear and Toughness\",\"datePublished\":\"2026-10-03T08:12:27+00:00\",\"dateModified\":\"2026-10-15T17:13:45+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/\"},\"wordCount\":1725,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png\",\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/\",\"name\":\"P\\\/M Tool Steel Properties, Wear and Toughness\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png\",\"datePublished\":\"2026-10-03T08:12:27+00:00\",\"dateModified\":\"2026-10-15T17:13:45+00:00\",\"description\":\"Carbide size, crossed-cylinder wear, Charpy impact and grinding ratios for P\\\/M and CPM tool steel against the conventional grades of the same type.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-tool-steel-properties\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"P\\\/M Tool Steel Properties, Carbide Size, Wear and Toughness\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Propriedades de A\u00e7o Ferramenta P\/M, Desgaste e Tenacidade","description":"Tamanho de carboneto, desgaste em cilindros cruzados, impacto Charpy e \u00edndices de retifica\u00e7\u00e3o para a\u00e7o ferramenta P\/M e CPM frente aos graus convencionais do mesmo tipo.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/pm-tool-steel-properties\/","og_locale":"pt_BR","og_type":"article","og_title":"P\/M Tool Steel Properties, Carbide Size, Wear and Toughness","og_description":"Carbide size, crossed-cylinder wear, Charpy impact and grinding ratios for P\/M and CPM tool steel against the conventional grades of the same type.","og_url":"https:\/\/aobosteel.com\/pt\/pm-tool-steel-properties\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T17:13:45+00:00","og_image":[{"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"9 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"P\/M Tool Steel Properties, Carbide Size, Wear and Toughness","datePublished":"2026-10-03T08:12:27+00:00","dateModified":"2026-10-15T17:13:45+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/"},"wordCount":1725,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png","inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/","url":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/","name":"Propriedades de A\u00e7o Ferramenta P\/M, Desgaste e Tenacidade","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png","datePublished":"2026-10-03T08:12:27+00:00","dateModified":"2026-10-15T17:13:45+00:00","description":"Tamanho de carboneto, desgaste em cilindros cruzados, impacto Charpy e \u00edndices de retifica\u00e7\u00e3o para a\u00e7o ferramenta P\/M e CPM frente aos graus convencionais do mesmo tipo.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/pm-tool-steel-properties\/"]}]},{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-Tool-Steel-fig-3-carbide-size-distribution.png"},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/pm-tool-steel-properties\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"P\/M Tool Steel Properties, Carbide Size, Wear and Toughness"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"P\/M Tool Steel Properties, Carbide Size, Wear and Toughness Powder metallurgy tool steel is bought for one reason. The carbides in it are small and evenly spread instead of coarse and banded. Everything else about the grade follows from that, and the charts on this page measure it. The median primary carbide in CPM T15&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"P\/M Tool Steel Properties, Carbide Size, Wear and Toughness Powder metallurgy tool steel is bought for one reason. The carbides in it are small and evenly spread instead of coarse and banded. Everything else about the grade follows from that, and the charts on this page measure it. The median primary carbide in CPM T15&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20798","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=20798"}],"version-history":[{"count":4,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20798\/revisions"}],"predecessor-version":[{"id":22612,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20798\/revisions\/22612"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=20798"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}