{"id":20748,"date":"2026-10-03T08:06:12","date_gmt":"2026-10-03T00:06:12","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20748"},"modified":"2026-10-16T01:11:08","modified_gmt":"2026-10-15T17:11:08","slug":"tool-steel-bar-delivery-condition","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/tool-steel-bar-delivery-condition\/","title":{"rendered":"Condi\u00e7\u00e3o de entrega da barra de a\u00e7o ferramenta, laminado e recozido"},"content":{"rendered":"<h1 class=\"wp-block-heading\">Condi\u00e7\u00e3o de entrega da barra de a\u00e7o ferramenta, laminado e recozido<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">Duas barras do mesmo grau de a\u00e7o ferramenta podem chegar com estruturas diferentes e durezas diferentes, e a diferen\u00e7a \u00e9 decidida por como a barra resfriou ap\u00f3s o \u00faltimo passe de lamina\u00e7\u00e3o e por qual recozimento foi aplicado depois. Esta p\u00e1gina re\u00fane as estruturas laminadas de L6, S4, S5 e L1, a rede de carbonetos nos contornos de gr\u00e3o que um grau de alto carbono adquire na linha de lamina\u00e7\u00e3o, e as estruturas recozidas de usina contra totalmente recozidas de W4, W1 e H26, para que a condi\u00e7\u00e3o de entrega no certificado possa ser comparada com a estrutura na barra.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Do que depende a estrutura laminada<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A estrutura que uma barra de a\u00e7o ferramenta apresenta ao sair da linha de lamina\u00e7\u00e3o \u00e9 definida pela temperabilidade do grau e pela taxa de resfriamento que a barra sofreu ap\u00f3s o \u00faltimo passe. Um grau resistente ao choque com teor moderado de liga pode sair de ambas as formas, e as duas placas S4 abaixo s\u00e3o o mesmo grau resfriado a duas taxas diferentes. O contato t\u00e9rmico deficiente com o leito de resfriamento deixa a mais lenta como ferrita e perlita, e um resfriamento mais r\u00e1pido a leva para a faixa de bainita e martensita e deixa a barra mais dura e mais sens\u00edvel a trincas do que o certificado sugere.<\/p>\n\n\n\n<div class=\"wp-block-columns is-layout-flex wp-container-core-columns-is-layout-7387b849 wp-block-columns-is-layout-flex\">\n<div class=\"wp-block-column is-layout-flow wp-block-column-is-layout-flow\">\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg\" alt=\"AISI S4 tool steel as-rolled with ferrite and pearlite after slow cooling, 4% picral, 500x\"\/><figcaption class=\"wp-element-caption\">Fig. 12. S4 laminado, ferrita em branco com perlita em uma barra que resfriou lentamente ap\u00f3s a lamina\u00e7\u00e3o. 4% picral, 500x.<\/figcaption><\/figure>\n<\/div>\n\n\n\n<div class=\"wp-block-column is-layout-flow wp-block-column-is-layout-flow\">\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-13-s4-faster-cooled.jpg\" alt=\"AISI S4 tool steel as-rolled and faster cooled, bainite and martensite, 4% picral, 500x\"\/><figcaption class=\"wp-element-caption\">Fig. 13. A mesma barra laminada S4 resfriada a uma taxa mais r\u00e1pida, resultando em bainita e martensita em manchas sem tra\u00e7os, em vez da ferrita e perlita acima. 4% picral, 500x.<\/figcaption><\/figure>\n<\/div>\n\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">A mesma divis\u00e3o aparece em toda a fam\u00edlia. L6 e S5 chegam como bainita e martensita de um resfriamento normal de lamina\u00e7\u00e3o, e as placas abaixo s\u00e3o a leitura esperada de uma inspe\u00e7\u00e3o de recebimento desses dois graus.<\/p>\n\n\n\n<div class=\"wp-block-columns is-layout-flex wp-container-core-columns-is-layout-7387b849 wp-block-columns-is-layout-flex\">\n<div class=\"wp-block-column is-layout-flow wp-block-column-is-layout-flow\">\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-11-l6-as-rolled.jpg\" alt=\"AISI L6 tool steel as-rolled with bainite and martensite, 2% nital, 500x\"\/><figcaption class=\"wp-element-caption\">Fig. 11. L6 laminado, bainita e martensita em branco. 2% nital, 500x.<\/figcaption><\/figure>\n<\/div>\n\n\n\n<div class=\"wp-block-column is-layout-flow wp-block-column-is-layout-flow\">\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-14-s5-as-rolled.jpg\" alt=\"AISI S5 tool steel as-rolled with bainite and martensite, 2% nital, 500x\"\/><figcaption class=\"wp-element-caption\">Fig. 14. S5 laminado, bainita e martensita em branco. 2% nital, 500x.<\/figcaption><\/figure>\n<\/div>\n\n<\/div>\n\n\n\n<h2 class=\"wp-block-heading\">Redes de carbonetos nos contornos de gr\u00e3o provenientes da linha de lamina\u00e7\u00e3o<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Uma estrutura mais s\u00e9ria que uma varia\u00e7\u00e3o de dureza \u00e9 a rede de carbonetos. Alguns a\u00e7os ferramenta, em particular os graus de trabalho a quente com 5% de cromo e os a\u00e7os para moldes pl\u00e1sticos com 12% de cromo, formam redes nos contornos de gr\u00e3o austen\u00edticos pr\u00e9vios durante o trabalho a quente, e os graus de alto carbono temper\u00e1veis em \u00e1gua as formam quando a barra resfria atrav\u00e9s da faixa de precipita\u00e7\u00e3o de carbonetos ap\u00f3s o \u00faltimo passe. L1 laminado e resfriado deixa perlita com uma rede de cementita nos contornos, que o ataque com picrato de s\u00f3dio alcalino colore para que a rede possa ser tra\u00e7ada, e um grau temper\u00e1vel em \u00e1gua com 1,31% C mostra a mesma rede ap\u00f3s resfriamento a partir da temperatura de lamina\u00e7\u00e3o.<\/p>\n\n\n\n<div class=\"wp-block-columns is-layout-flex wp-container-core-columns-is-layout-7387b849 wp-block-columns-is-layout-flex\">\n<div class=\"wp-block-column is-layout-flow wp-block-column-is-layout-flow\">\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-16-l1-cementite-network.jpg\" alt=\"AISI L1 tool steel as-rolled, pearlite with grain boundary cementite network, 100x\"\/><figcaption class=\"wp-element-caption\">Fig. 16. L1 laminado, perlita com uma rede de cementita nos contornos de gr\u00e3o, colorida com picrato de s\u00f3dio alcalino em ebuli\u00e7\u00e3o. 100x.<\/figcaption><\/figure>\n<\/div>\n\n\n\n<div class=\"wp-block-column is-layout-flow wp-block-column-is-layout-flow\">\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-19-rolling-carbide-network.jpg\" alt=\"Grain boundary carbide networks after cooling from the hot rolling temperature, alkaline sodium picrate, 500x\"\/><figcaption class=\"wp-element-caption\">Fig. 19. Redes de carbonetos nos contornos de gr\u00e3o em um grau temper\u00e1vel em \u00e1gua de alto carbono (1,31% C, 0,35% Mn, 0,25% Si) ap\u00f3s resfriamento a partir da temperatura de lamina\u00e7\u00e3o a quente, reveladas com picrato de s\u00f3dio alcalino a 90 &#176;C por 60 s. 500x.<\/figcaption><\/figure>\n<\/div>\n\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">Uma rede como essa \u00e9 dif\u00edcil de remover durante o recozimento e prejudica a ductilidade \u00e0 tra\u00e7\u00e3o e a tenacidade mesmo quando \u00e9 apenas semicont\u00ednua, raz\u00e3o pela qual os graus que a formam s\u00e3o normalizados antes de serem recozidos. Fios de carboneto de liga complexo s\u00e3o a outra estrutura prejudicial da linha de lamina\u00e7\u00e3o, e um exemplo no a\u00e7o de trabalho a quente H13 est\u00e1 na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-microstructure\/\">microestrutura do a\u00e7o ferramenta<\/a> p\u00e1gina. Se uma barra chega com uma rede pesada e as pe\u00e7as feitas a partir dela trincam em servi\u00e7o, a rede \u00e9 a primeira estrutura a ser examinada, e ela \u00e9 verificada na barra recozida antes de o material ser liberado para a oficina.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Recozido de usina contra totalmente recozido<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Uma entrega descrita como recozida pode significar duas coisas diferentes, e a diferen\u00e7a merece uma pergunta na fase de pedido. Um recozimento de usina \u00e9 um recozimento subcr\u00edtico realizado na usina para levar a barra a uma condi\u00e7\u00e3o usin\u00e1vel, e n\u00e3o dissolve a perlita lamelar que a linha de lamina\u00e7\u00e3o deixou. Um recozimento pleno austenitiza o a\u00e7o e o resfria atrav\u00e9s da faixa de transforma\u00e7\u00e3o lentamente o suficiente para que o carboneto se esferoidize completamente. As tr\u00eas placas abaixo s\u00e3o a mesma fam\u00edlia em ambas as condi\u00e7\u00f5es, e os valores de dureza correspondentes s\u00e3o 187 HB para o W4 recozido de usina contra 170 HB para o W4 totalmente recozido da mesma composi\u00e7\u00e3o qu\u00edmica.<\/p>\n\n\n\n<div class=\"wp-block-columns is-layout-flex wp-container-core-columns-is-layout-7387b849 wp-block-columns-is-layout-flex\">\n<div class=\"wp-block-column is-layout-flow wp-block-column-is-layout-flow\">\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-22-w4-mill-annealed.jpg\" alt=\"AISI W4 tool steel as received mill annealed, spheroidal cementite with lamellar pearlite, 187 HB, 1000x\"\/><figcaption class=\"wp-element-caption\">Fig. 22. W4 (0,98% C, 0,74% Mn, 0,14% Cr, 0,19% Ni) como recebido, recozido de usina, 187 HB. Cementita esferoidal em matriz ferr\u00edtica com uma quantidade consider\u00e1vel de perlita lamelar ainda presente. 4% picral, 1000x.<\/figcaption><\/figure>\n<\/div>\n\n\n\n<div class=\"wp-block-column is-layout-flow wp-block-column-is-layout-flow\">\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-23-w4-full-annealed.jpg\" alt=\"AISI W4 tool steel fully annealed, spheroidal cementite with no lamellar pearlite, 170 HB, 1000x\"\/><figcaption class=\"wp-element-caption\">Fig. 23. W4 (0,96% C, 0,66% Mn, 0,23% Cr) como recebido, totalmente recozido, 170 HB. Cementita esferoidal em matriz ferr\u00edtica sem constituinte lamelar presente. 4% picral, 1000x.<\/figcaption><\/figure>\n<\/div>\n\n<\/div>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-24-w1-mill-annealed.jpg\" alt=\"AISI W1 tool steel as received mill annealed, lamellar pearlite and spheroidal cementite, 170 HB, 3% nital, 1000x\"\/><figcaption class=\"wp-element-caption\">Fig. 24. W1 (0,94% C, 0,21% Mn) como recebido, recozido de usina, 170 HB. Uma mistura de perlita lamelar e cementita esferoidal em matriz ferr\u00edtica, com algumas part\u00edculas grandes de carboneto globular. 3% nital, 1000x.<\/figcaption><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">A consequ\u00eancia pr\u00e1tica \u00e9 que uma barra recozida de usina usina-se com acabamento diferente, e responder\u00e1 ao ciclo de t\u00eampera de forma um pouco diferente porque parte de seu carboneto ainda \u00e9 lamelar. Para um bloco de matriz que ser\u00e1 desbastado e depois temperado, a diferen\u00e7a raramente importa. Para uma pe\u00e7a com muita usinagem ou uma dimens\u00e3o apertada antes da t\u00eampera, importa, e a estrutura a solicitar \u00e9 um recozimento pleno. A mesma distin\u00e7\u00e3o est\u00e1 por tr\u00e1s do recozimento para esferoidiza\u00e7\u00e3o na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-annealing-normalizing-temperature-chart\/\">gr\u00e1fico de recozimento e normaliza\u00e7\u00e3o<\/a> p\u00e1gina.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Dispers\u00e3o de carbonetos de liga em um grau de alta liga<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Os graus de alta liga temper\u00e1veis em \u00e1gua e de trabalho a quente n\u00e3o ret\u00eam perlita lamelar na condi\u00e7\u00e3o recozida. O H26 recozido a partir de 900 &#176;C com resfriamento controlado at\u00e9 650 &#176;C resulta em 22 a 23 HRC como uma dispers\u00e3o de part\u00edculas finas de carboneto de liga em matriz ferr\u00edtica, que \u00e9 a estrutura que torna o grau usin\u00e1vel. \u00c9 lido com picral e HCl em vez de nital, porque o carboneto est\u00e1 suficientemente fino para que um ataque simples com nital n\u00e3o o separe da matriz.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-36-h26-annealed.jpg\" alt=\"AISI H26 tool steel annealed, fine alloy carbide dispersion in ferrite, 22 to 23 HRC, 500x\"\/><figcaption class=\"wp-element-caption\">Fig. 36. H26 recozido por austenitiza\u00e7\u00e3o a 900 &#176;C e resfriamento a 8,5 &#176;C\/h at\u00e9 650 &#176;C, depois resfriamento ao ar, 22 a 23 HRC. Uma dispers\u00e3o de part\u00edculas finas de carboneto de liga em matriz ferr\u00edtica. Picral com HCl, 10 s, 500x.<\/figcaption><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">Leitura de uma entrega na amplia\u00e7\u00e3o correta<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A \u00faltima placa \u00e9 a raz\u00e3o pela qual uma verifica\u00e7\u00e3o de entrega \u00e9 feita a 500x ou 1000x em vez de 100x. O mesmo corpo de prova de A10 recozido de usina que apresenta uma estrutura resolv\u00edvel em alta amplia\u00e7\u00e3o mostra quase nada al\u00e9m de um campo cinza a 100x, e uma verifica\u00e7\u00e3o lida nessa amplia\u00e7\u00e3o aprovar\u00e1 uma barra cujo carboneto \u00e9 mais grosso do que a especifica\u00e7\u00e3o permite. A verifica\u00e7\u00e3o de rotina \u00e9 uma se\u00e7\u00e3o transversal a 500x com o ataque que o grau normalmente \u00e9 lido, e a se\u00e7\u00e3o longitudinal \u00e9 adicionada quando a quest\u00e3o \u00e9 bandeamento ou uma rede, em vez do tamanho do carboneto.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-34-a10-as-received.jpg\" alt=\"AISI A10 tool steel as received mill annealed at 100x, structure poorly resolved, nital\"\/><figcaption class=\"wp-element-caption\">Fig. 34. A\u00e7o ferramenta A10 como recebido, recozido de usina, se\u00e7\u00e3o tomada transversalmente \u00e0 dire\u00e7\u00e3o de lamina\u00e7\u00e3o. A 100x a estrutura \u00e9 mal resolvida, raz\u00e3o pela qual uma verifica\u00e7\u00e3o de entrega \u00e9 lida a 500x ou 1000x em vez de em baixa amplia\u00e7\u00e3o. Nital, 100x.<\/figcaption><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Os ataques para cada uma dessas estruturas est\u00e3o listados na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-microstructure\/\">microestrutura do a\u00e7o ferramenta<\/a> p\u00e1gina, e os ciclos de forno que produzem uma estrutura totalmente esferoidizada est\u00e3o na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-annealing-normalizing-temperature-chart\/\">tabela de temperaturas de recozimento e normaliza\u00e7\u00e3o<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Compilado do ASM Handbook, Volume 9, Metallography and Microstructures, artigo Metallographic Techniques for Tool Steels de George F. Vander Voort, ASM International, 2004 (se\u00e7\u00f5es de microestrutura laminada e recozida, Fig. 11 a Fig. 14, Fig. 16, 19, 22 a 24, 34 e 36). Cada legenda foi lida da camada de texto pesquis\u00e1vel do arquivo e verificada contra a placa impressa, e cada placa foi recortada do arquivo a 1,5 vezes sua largura em pixels impressa. As placas s\u00e3o um resumo de refer\u00eancia da pr\u00e1tica publicada, e n\u00e3o uma especifica\u00e7\u00e3o da Aobo Steel, portanto confirme a condi\u00e7\u00e3o de entrega, o estado de recozimento e a dureza contra o certificado de ensaio do material antes de fazer um pedido.<\/p>","protected":false},"excerpt":{"rendered":"<p>Tool Steel Bar Delivery Condition, As-Rolled and Annealed Two bars of the same tool steel grade can arrive with different structures and different hardnesses, and the difference is decided by how the bar cooled after the last rolling pass and by which anneal it was given afterwards. This page collects the as-rolled structures of L6, [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20748","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Tool Steel Bar Delivery Condition | Mill Annealed Structure<\/title>\n<meta name=\"description\" content=\"As-rolled and annealed tool steel structures, showing how the cooling rate after rolling and the anneal that follows change the structure and the delivery hardness.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/tool-steel-bar-delivery-condition\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Tool Steel Bar Delivery Condition, As-Rolled and Annealed\" \/>\n<meta property=\"og:description\" content=\"As-rolled and annealed tool steel structures, showing how the cooling rate after rolling and the anneal that follows change the structure and the delivery hardness.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/tool-steel-bar-delivery-condition\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T17:11:08+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"6 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Tool Steel Bar Delivery Condition, As-Rolled and Annealed\",\"datePublished\":\"2026-10-03T00:06:12+00:00\",\"dateModified\":\"2026-10-15T17:11:08+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/\"},\"wordCount\":1289,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg\",\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/\",\"name\":\"Tool Steel Bar Delivery Condition | Mill Annealed Structure\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg\",\"datePublished\":\"2026-10-03T00:06:12+00:00\",\"dateModified\":\"2026-10-15T17:11:08+00:00\",\"description\":\"As-rolled and annealed tool steel structures, showing how the cooling rate after rolling and the anneal that follows change the structure and the delivery hardness.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-bar-delivery-condition\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Tool Steel Bar Delivery Condition, As-Rolled and Annealed\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Condi\u00e7\u00e3o de Entrega de Barra de A\u00e7o Ferramenta | Estrutura Recozida em Forno","description":"Estruturas de a\u00e7o ferramenta laminado e recozido, mostrando como a taxa de resfriamento ap\u00f3s lamina\u00e7\u00e3o e o recozimento subsequente alteram a estrutura e a dureza de entrega.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/tool-steel-bar-delivery-condition\/","og_locale":"pt_BR","og_type":"article","og_title":"Tool Steel Bar Delivery Condition, As-Rolled and Annealed","og_description":"As-rolled and annealed tool steel structures, showing how the cooling rate after rolling and the anneal that follows change the structure and the delivery hardness.","og_url":"https:\/\/aobosteel.com\/pt\/tool-steel-bar-delivery-condition\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T17:11:08+00:00","og_image":[{"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"6 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Tool Steel Bar Delivery Condition, As-Rolled and Annealed","datePublished":"2026-10-03T00:06:12+00:00","dateModified":"2026-10-15T17:11:08+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/"},"wordCount":1289,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg","inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/","url":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/","name":"Condi\u00e7\u00e3o de Entrega de Barra de A\u00e7o Ferramenta | Estrutura Recozida em Forno","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg","datePublished":"2026-10-03T00:06:12+00:00","dateModified":"2026-10-15T17:11:08+00:00","description":"Estruturas de a\u00e7o ferramenta laminado e recozido, mostrando como a taxa de resfriamento ap\u00f3s lamina\u00e7\u00e3o e o recozimento subsequente alteram a estrutura e a dureza de entrega.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/"]}]},{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Microstructure-delivery-fig-12-s4-as-rolled.jpg"},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-bar-delivery-condition\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Tool Steel Bar Delivery Condition, As-Rolled and Annealed"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Tool Steel Bar Delivery Condition, As-Rolled and Annealed Two bars of the same tool steel grade can arrive with different structures and different hardnesses, and the difference is decided by how the bar cooled after the last rolling pass and by which anneal it was given afterwards. This page collects the as-rolled structures of L6,&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Tool Steel Bar Delivery Condition, As-Rolled and Annealed Two bars of the same tool steel grade can arrive with different structures and different hardnesses, and the difference is decided by how the bar cooled after the last rolling pass and by which anneal it was given afterwards. This page collects the as-rolled structures of L6,&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20748","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=20748"}],"version-history":[{"count":2,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20748\/revisions"}],"predecessor-version":[{"id":22605,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20748\/revisions\/22605"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=20748"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}