{"id":20579,"date":"2026-10-02T15:05:33","date_gmt":"2026-10-02T07:05:33","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20579"},"modified":"2026-10-16T00:54:37","modified_gmt":"2026-10-15T16:54:37","slug":"pm-high-speed-steel-composition","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/pm-high-speed-steel-composition\/","title":{"rendered":"Graus de A\u00e7o R\u00e1pido PM e Sua Composi\u00e7\u00e3o Qu\u00edmica"},"content":{"rendered":"<h1 class=\"wp-block-heading\">Graus de A\u00e7o R\u00e1pido PM e Sua Composi\u00e7\u00e3o Qu\u00edmica<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">O a\u00e7o r\u00e1pido de metalurgia do p\u00f3 \u00e9 produzido pela atomiza\u00e7\u00e3o do fundido em p\u00f3 e sua consolida\u00e7\u00e3o, de modo que os carbonetos que ele cont\u00e9m s\u00e3o finos e uniformemente distribu\u00eddos, em vez de grosseiros e em bandas. A tabela abaixo lista os graus PM que aparecem com mais frequ\u00eancia em documentos de ferramentaria e de compras e a composi\u00e7\u00e3o qu\u00edmica de cada um.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">O que a rota do p\u00f3 muda<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Um a\u00e7o r\u00e1pido convencional \u00e9 fundido em lingote, e os carbonetos que se formam \u00e0 medida que o lingote solidifica s\u00e3o grosseiros e disp\u00f5em-se em bandas. A metalurgia do p\u00f3 segue um caminho diferente. O fundido \u00e9 atomizado em p\u00f3 e o p\u00f3 \u00e9 consolidado, de modo que uma liga com a mesma an\u00e1lise acaba com carbonetos de apenas alguns micr\u00f3metros de di\u00e2metro, distribu\u00eddos uniformemente pela matriz em vez de agrupados em bandas. Os resultados pr\u00e1ticos s\u00e3o <a href=\"https:\/\/aobosteel.com\/pt\/pm-tool-steel-properties\/\">melhor retificabilidade e melhor tenacidade na mesma dureza<\/a>, e uma varia\u00e7\u00e3o mais estreita na vida \u00fatil da ferramenta de um lote de a\u00e7o para o seguinte.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\u00c9 por isso que as composi\u00e7\u00f5es abaixo parecem familiares. O CPM M2 e o CPM M42 t\u00eam a an\u00e1lise dos a\u00e7os r\u00e1pidos convencionais M2 e M42, e a diferen\u00e7a pela qual o comprador paga \u00e9 o tamanho do carboneto e n\u00e3o uma liga diferente. <a href=\"https:\/\/aobosteel.com\/pt\/pm-tool-steel-composition-chart\/\">Os graus ABM vendidos sob o nome ASP e os graus HAP<\/a> seguem a mesma l\u00f3gica, com maior teor de carbono e van\u00e1dio nos graus destinados ao trabalho de corte mais severo.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Graus e composi\u00e7\u00e3o qu\u00edmica<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A tabela re\u00fane os graus PM que aparecem com mais frequ\u00eancia em desenhos de ferramentaria e em documentos de compras, agrupados pelo pa\u00eds cujas usinas os desenvolveram. Um tra\u00e7o marca uma c\u00e9lula que a fonte deixa vazia.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Composi\u00e7\u00e3o qu\u00edmica dos graus de a\u00e7o r\u00e1pido PM, percentual em massa<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Grau<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pa\u00eds<\/th><th class=\"has-text-align-left\" data-align=\"left\">C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Cr<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mo<\/th><th class=\"has-text-align-left\" data-align=\"left\">W<\/th><th class=\"has-text-align-left\" data-align=\"left\">Co<\/th><th class=\"has-text-align-left\" data-align=\"left\">V<\/th><th class=\"has-text-align-left\" data-align=\"left\">Nb<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">ASP2017<\/td><td class=\"has-text-align-left\" data-align=\"left\">Fran\u00e7a<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">ASP2023<\/td><td class=\"has-text-align-left\" data-align=\"left\">Fran\u00e7a<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.28<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">ASP2030<\/td><td class=\"has-text-align-left\" data-align=\"left\">Fran\u00e7a<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.28<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">ASP2053<\/td><td class=\"has-text-align-left\" data-align=\"left\">Fran\u00e7a<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.45<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">ASP2060<\/td><td class=\"has-text-align-left\" data-align=\"left\">Fran\u00e7a<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">CPM M2<\/td><td class=\"has-text-align-left\" data-align=\"left\">Estados Unidos<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">CPM M42<\/td><td class=\"has-text-align-left\" data-align=\"left\">Estados Unidos<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">HAP10<\/td><td class=\"has-text-align-left\" data-align=\"left\">Jap\u00e3o<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">6<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">HAP20<\/td><td class=\"has-text-align-left\" data-align=\"left\">Jap\u00e3o<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">HAP40<\/td><td class=\"has-text-align-left\" data-align=\"left\">Jap\u00e3o<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">HAP50<\/td><td class=\"has-text-align-left\" data-align=\"left\">Jap\u00e3o<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">6<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">HAP70<\/td><td class=\"has-text-align-left\" data-align=\"left\">Jap\u00e3o<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">HAP72<\/td><td class=\"has-text-align-left\" data-align=\"left\">Jap\u00e3o<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">FT15<\/td><td class=\"has-text-align-left\" data-align=\"left\">China<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">&lt;1<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">FR71<\/td><td class=\"has-text-align-left\" data-align=\"left\">China<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">GF1<\/td><td class=\"has-text-align-left\" data-align=\"left\">China<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.85<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">18<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">GF2<\/td><td class=\"has-text-align-left\" data-align=\"left\">China<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">6<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">GF3<\/td><td class=\"has-text-align-left\" data-align=\"left\">China<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">4<\/td><td class=\"has-text-align-left\" data-align=\"left\">5<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">9<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8212;<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fonte, \u5200\u5177\u6750\u6599\u901f\u67e5\u624b\u518c, Tabela 2-21, Graus de a\u00e7o r\u00e1pido PM nacionais e estrangeiros e sua composi\u00e7\u00e3o qu\u00edmica, p\u00e1gina impressa 33. Todos os valores s\u00e3o percentuais em massa. Cada n\u00famero foi lido de uma imagem renderizada da p\u00e1gina impressa e conferido linha por linha. Este \u00e9 um resumo de refer\u00eancia da pr\u00e1tica publicada e n\u00e3o uma especifica\u00e7\u00e3o da Aobo Steel.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Notas da tabela. Os graus s\u00e3o agrupados pelo pa\u00eds cujas usinas os desenvolveram, na ordem em que a fonte os imprime, e o valor de ni\u00f3bio \u00e9 impresso uma vez para cada grupo. Um tra\u00e7o \u00e9 uma c\u00e9lula que a fonte deixa vazia, o que na coluna de cobalto marca um grau isento de cobalto. O valor de cromo para o ASP2017 \u00e9 impresso como 4,2 na fonte e como 4,0 na ficha t\u00e9cnica do pr\u00f3prio fabricante; ambas as leituras s\u00e3o da mesma an\u00e1lise nominal. As an\u00e1lises nominais variam por fabricante e por revis\u00e3o, portanto confirme a an\u00e1lise da corrida no certificado da usina antes de um grau ser inclu\u00eddo em uma especifica\u00e7\u00e3o de compra.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Leitura das colunas de composi\u00e7\u00e3o<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O carbono fica entre 0,8 e 2,45 por cento em toda a tabela e \u00e9 o primeiro n\u00famero a ser lido, porque define o volume de carboneto que o a\u00e7o pode formar e, portanto, o limite de dureza. Os graus isentos de cobalto s\u00e3o os que est\u00e3o no meio dessa faixa, e os graus com mais de 2 por cento de carbono s\u00e3o os vendidos para o trabalho de corte mais abrasivo.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O van\u00e1dio \u00e9 a coluna que separa um grau PM de uso geral de um grau de desgaste. Ele vai de 1 por cento no ASP2017 a 8 por cento no ASP2053, e quanto mais alto, mais dif\u00edcil se torna retificar o a\u00e7o, que \u00e9 a troca que a rota do p\u00f3 foi inventada para suavizar. O tungst\u00eanio e o molibd\u00eanio formam os carbonetos duros e s\u00e3o lidos em conjunto, pois um grau com teor alto de um geralmente tem teor baixo do outro.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O cobalto eleva a dureza a quente, raz\u00e3o pela qual aparece em 8 a 12 por cento nos graus usados no corte em alta velocidade de materiais tenazes e est\u00e1 vazio nos graus vendidos para trabalho a frio e para moldes de pl\u00e1stico. O ni\u00f3bio aparece uma vez na tabela, a 1 por cento no grupo ASP, onde \u00e9 adicionado para controlar o crescimento de gr\u00e3o durante a consolida\u00e7\u00e3o.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Dados de refer\u00eancia relacionados<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O CPM M2 e o CPM M42 mant\u00eam a an\u00e1lise dos graus convencionais fornecidos como <a href=\"https:\/\/aobosteel.com\/pt\/m2-tool-steel\/\">A\u00e7o ferramenta M2<\/a> e <a href=\"https:\/\/aobosteel.com\/pt\/m42-tool-steel\/\">A\u00e7o ferramenta M42<\/a>. As faixas de composi\u00e7\u00e3o dos graus convencionais com os quais esses a\u00e7os PM s\u00e3o comparados est\u00e3o listadas na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-composition-chart\/\">Tabela de composi\u00e7\u00e3o de a\u00e7os para ferramentas<\/a>, e a diferen\u00e7a microestrutural entre as duas rotas \u00e9 apresentada em <a href=\"https:\/\/aobosteel.com\/pt\/blog\/pm-vs-conventional-tool-steel\/\">PM versus a\u00e7o ferramenta convencional<\/a>.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>Tabela de composi\u00e7\u00e3o do a\u00e7o r\u00e1pido PM, PDF para impress\u00e3o<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">Composi\u00e7\u00e3o qu\u00edmica dos graus de a\u00e7o r\u00e1pido ASP, CPM, HAP e PM chin\u00eas, em um \u00fanico PDF com nossos dados de contato.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-PM-High-Speed-Steel-Composition.pdf\">Baixar PDF<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">Compilado de \u5200\u5177\u6750\u6599\u901f\u67e5\u624b\u518c, Tabela 2-21 na p\u00e1gina impressa 33. Cada valor foi lido de uma imagem renderizada da p\u00e1gina impressa e verificado linha por linha. A tabela \u00e9 um resumo de refer\u00eancia da pr\u00e1tica publicada, e n\u00e3o uma especifica\u00e7\u00e3o da Aobo Steel, portanto confirme a an\u00e1lise de fus\u00e3o no certificado do laminador antes que os dados sejam inseridos em uma folha de processo.<\/p>","protected":false},"excerpt":{"rendered":"<p>PM High Speed Steel Grades and Their Chemical Composition Powder metallurgy high speed steel is made by atomising the melt into powder and consolidating it, so the carbides it carries are fine and evenly spread instead of coarse and banded. The table below lists the PM grades that turn up most often in tool room [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20579","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>PM High Speed Steel Composition Chart (ASP, CPM, HAP Grades)<\/title>\n<meta name=\"description\" content=\"Chemical composition of powder metallurgy high speed steel grades, Erasteel ASP, CPM, HAP and Chinese PM series, with C, Cr, Mo, W, Co, V and Nb in mass percent.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/pm-high-speed-steel-composition\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"PM High Speed Steel Grades and Their Chemical Composition\" \/>\n<meta property=\"og:description\" content=\"Chemical composition of powder metallurgy high speed steel grades, Erasteel ASP, CPM, HAP and Chinese PM series, with C, Cr, Mo, W, Co, V and Nb in mass percent.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/pm-high-speed-steel-composition\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T16:54:37+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"4 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-high-speed-steel-composition\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-high-speed-steel-composition\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"PM High Speed Steel Grades and Their Chemical Composition\",\"datePublished\":\"2026-10-02T07:05:33+00:00\",\"dateModified\":\"2026-10-15T16:54:37+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-high-speed-steel-composition\\\/\"},\"wordCount\":853,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-high-speed-steel-composition\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/pm-high-speed-steel-composition\\\/\",\"name\":\"PM High Speed Steel Composition Chart (ASP, CPM, HAP Grades)\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-02T07:05:33+00:00\",\"dateModified\":\"2026-10-15T16:54:37+00:00\",\"description\":\"Chemical composition of powder metallurgy high speed steel grades, Erasteel ASP, CPM, HAP and Chinese PM series, with C, Cr, Mo, W, Co, V and Nb in mass percent.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-high-speed-steel-composition\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/pm-high-speed-steel-composition\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/pm-high-speed-steel-composition\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"PM High Speed Steel Grades and Their Chemical Composition\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Tabela de Composi\u00e7\u00e3o de A\u00e7o R\u00e1pido PM (Graus ASP, CPM, HAP)","description":"Composi\u00e7\u00e3o qu\u00edmica de graus de a\u00e7o r\u00e1pido metalurgia do p\u00f3, s\u00e9ries Erasteel ASP, CPM, HAP e PM chinesa, com C, Cr, Mo, W, Co, V e Nb em porcentagem de massa.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/pm-high-speed-steel-composition\/","og_locale":"pt_BR","og_type":"article","og_title":"PM High Speed Steel Grades and Their Chemical Composition","og_description":"Chemical composition of powder metallurgy high speed steel grades, Erasteel ASP, CPM, HAP and Chinese PM series, with C, Cr, Mo, W, Co, V and Nb in mass percent.","og_url":"https:\/\/aobosteel.com\/pt\/pm-high-speed-steel-composition\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T16:54:37+00:00","twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"4 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/pm-high-speed-steel-composition\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/pm-high-speed-steel-composition\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"PM High Speed Steel Grades and Their Chemical Composition","datePublished":"2026-10-02T07:05:33+00:00","dateModified":"2026-10-15T16:54:37+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/pm-high-speed-steel-composition\/"},"wordCount":853,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/pm-high-speed-steel-composition\/","url":"https:\/\/aobosteel.com\/pm-high-speed-steel-composition\/","name":"Tabela de Composi\u00e7\u00e3o de A\u00e7o R\u00e1pido PM (Graus ASP, CPM, HAP)","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-02T07:05:33+00:00","dateModified":"2026-10-15T16:54:37+00:00","description":"Composi\u00e7\u00e3o qu\u00edmica de graus de a\u00e7o r\u00e1pido metalurgia do p\u00f3, s\u00e9ries Erasteel ASP, CPM, HAP e PM chinesa, com C, Cr, Mo, W, Co, V e Nb em porcentagem de massa.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/pm-high-speed-steel-composition\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/pm-high-speed-steel-composition\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/pm-high-speed-steel-composition\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"PM High Speed Steel Grades and Their Chemical Composition"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"PM High Speed Steel Grades and Their Chemical Composition Powder metallurgy high speed steel is made by atomising the melt into powder and consolidating it, so the carbides it carries are fine and evenly spread instead of coarse and banded. The table below lists the PM grades that turn up most often in tool room&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"PM High Speed Steel Grades and Their Chemical Composition Powder metallurgy high speed steel is made by atomising the melt into powder and consolidating it, so the carbides it carries are fine and evenly spread instead of coarse and banded. The table below lists the PM grades that turn up most often in tool room&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20579","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=20579"}],"version-history":[{"count":4,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20579\/revisions"}],"predecessor-version":[{"id":22572,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20579\/revisions\/22572"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=20579"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}