{"id":20319,"date":"2026-09-30T06:08:56","date_gmt":"2026-09-29T22:08:56","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=20319"},"modified":"2026-11-09T08:08:01","modified_gmt":"2026-11-09T00:08:01","slug":"stainless-steel-corrosion-resistance-chart","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/stainless-steel-corrosion-resistance-chart\/","title":{"rendered":"Tabela de resist\u00eancia \u00e0 corros\u00e3o de a\u00e7os inoxid\u00e1veis"},"content":{"rendered":"<h1 class=\"wp-block-heading\">Tabela de resist\u00eancia \u00e0 corros\u00e3o de a\u00e7os inoxid\u00e1veis<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">Pontua\u00e7\u00e3o de resist\u00eancia \u00e0 corros\u00e3o para 48 graus de a\u00e7o inoxid\u00e1vel e a\u00e7o ferramenta, calculada a partir do cromo, molibd\u00eanio, tungst\u00eanio e nitrog\u00eanio deixados em solu\u00e7\u00e3o. Um resumo de refer\u00eancia da pr\u00e1tica publicada e n\u00e3o uma especifica\u00e7\u00e3o da Aobo Steel.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">O que a pontua\u00e7\u00e3o de resist\u00eancia \u00e0 corros\u00e3o mede<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A resist\u00eancia \u00e0 ferrugem em um a\u00e7o inoxid\u00e1vel vem do cromo que \u00e9 deixado em solu\u00e7\u00e3o na matriz. O elemento de liga que est\u00e1 combinado em carboneto n\u00e3o protege nada, e \u00e9 por isso que dois graus com o mesmo teor de cromo podem ficar muito distantes nesta escala. A pontua\u00e7\u00e3o na tabela \u00e9 a equa\u00e7\u00e3o de resist\u00eancia \u00e0 corros\u00e3o que a fonte desenvolveu a partir de seus pr\u00f3prios ensaios de corros\u00e3o, cromo mais 1,6 vezes molibd\u00eanio mais 0,8 vezes tungst\u00eanio mais 6 vezes nitrog\u00eanio, aplicada ao elemento de liga que est\u00e1 em solu\u00e7\u00e3o na temperatura de austenitiza\u00e7\u00e3o listada ao lado do grau. A contribui\u00e7\u00e3o do molibd\u00eanio, tungst\u00eanio e nitrog\u00eanio \u00e9 limitada, de modo que um grau n\u00e3o pode ultrapassar o teto com uma grande adi\u00e7\u00e3o de apenas um deles.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A linha divis\u00f3ria que a fonte utiliza para a palavra inoxid\u00e1vel \u00e9 uma pontua\u00e7\u00e3o de 11. Um grau com 11 ou mais passou no teste de corros\u00e3o que separa um a\u00e7o inoxid\u00e1vel de um a\u00e7o ferramenta, e um grau abaixo disso enferrujar\u00e1 no mesmo servi\u00e7o mesmo quando seu n\u00famero de cromo parecer saud\u00e1vel em um certificado de usina. Esse \u00fanico n\u00famero \u00e9 a raz\u00e3o pr\u00e1tica pela qual uma oficina de moldes recorre ao 420 ou 440C quando o pl\u00e1stico ou o fluido de corte \u00e9 agressivo, e permanece com o D2 ou A2 quando n\u00e3o \u00e9. \u00c9 tamb\u00e9m a raz\u00e3o pela qual um grau pode ser vendido como inoxid\u00e1vel e <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-pitting-corrosion\/\">ainda assim sofrer pitting em uma m\u00e1quina \u00famida<\/a>.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Resist\u00eancia \u00e0 corros\u00e3o de 48 a\u00e7os inoxid\u00e1veis e a\u00e7os ferramenta<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">Composi\u00e7\u00e3o e pontua\u00e7\u00e3o de resist\u00eancia \u00e0 corros\u00e3o por grau<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">A\u00e7o<\/th><th class=\"has-text-align-left\" data-align=\"left\">Austenitiza\u00e7\u00e3o (\u00b0F)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Cr (%)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mo (%)<\/th><th class=\"has-text-align-left\" data-align=\"left\">W (%)<\/th><th class=\"has-text-align-left\" data-align=\"left\">N (%)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pontua\u00e7\u00e3o<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Vanax<\/td><td class=\"has-text-align-left\" data-align=\"left\">1975<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">LC200N<\/td><td class=\"has-text-align-left\" data-align=\"left\">1875<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.28<\/td><td class=\"has-text-align-left\" data-align=\"left\">17.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M390<\/td><td class=\"has-text-align-left\" data-align=\"left\">2100<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S110V<\/td><td class=\"has-text-align-left\" data-align=\"left\">2150<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">15.1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">BD1N<\/td><td class=\"has-text-align-left\" data-align=\"left\">1925<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.13<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">440A<\/td><td class=\"has-text-align-left\" data-align=\"left\">1900<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">14.2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">14C28N<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.11<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S45VN<\/td><td class=\"has-text-align-left\" data-align=\"left\">1950<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.7<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">N690<\/td><td class=\"has-text-align-left\" data-align=\"left\">1925<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">BD1<\/td><td class=\"has-text-align-left\" data-align=\"left\">1900<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">VG-10<\/td><td class=\"has-text-align-left\" data-align=\"left\">1975<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S35VN<\/td><td class=\"has-text-align-left\" data-align=\"left\">1950<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">420<\/td><td class=\"has-text-align-left\" data-align=\"left\">1900<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Super Gold2<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">13.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Elmax<\/td><td class=\"has-text-align-left\" data-align=\"left\">1975<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S30V<\/td><td class=\"has-text-align-left\" data-align=\"left\">1950<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AUS-6<\/td><td class=\"has-text-align-left\" data-align=\"left\">1925<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S125V<\/td><td class=\"has-text-align-left\" data-align=\"left\">2125<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">420HC<\/td><td class=\"has-text-align-left\" data-align=\"left\">1900<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">440C<\/td><td class=\"has-text-align-left\" data-align=\"left\">1875<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Niolox<\/td><td class=\"has-text-align-left\" data-align=\"left\">1925<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S90V<\/td><td class=\"has-text-align-left\" data-align=\"left\">2125<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nitro-V<\/td><td class=\"has-text-align-left\" data-align=\"left\">1900<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.11<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AUS-8<\/td><td class=\"has-text-align-left\" data-align=\"left\">1925<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8Cr13MoV<\/td><td class=\"has-text-align-left\" data-align=\"left\">1925<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">154CM<\/td><td class=\"has-text-align-left\" data-align=\"left\">1950<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">12.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">AEB-L<\/td><td class=\"has-text-align-left\" data-align=\"left\">1950<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.7<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S60V<\/td><td class=\"has-text-align-left\" data-align=\"left\">2050<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.6<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">19C27<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">11.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">XHP<\/td><td class=\"has-text-align-left\" data-align=\"left\">1925<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.6<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A8 Mod<\/td><td class=\"has-text-align-left\" data-align=\"left\">1875<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.6<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">3V<\/td><td class=\"has-text-align-left\" data-align=\"left\">1975<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">CruWear<\/td><td class=\"has-text-align-left\" data-align=\"left\">1950<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">ZDP-189<\/td><td class=\"has-text-align-left\" data-align=\"left\">1875<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">K190<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2<\/td><td class=\"has-text-align-left\" data-align=\"left\">1850<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Maxamet<\/td><td class=\"has-text-align-left\" data-align=\"left\">2100<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Vanadis 8<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Vanadis 4E<\/td><td class=\"has-text-align-left\" data-align=\"left\">1875<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">7.1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M2<\/td><td class=\"has-text-align-left\" data-align=\"left\">2100<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">K390<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.7<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M4<\/td><td class=\"has-text-align-left\" data-align=\"left\">2100<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.6<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10V<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.7<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">1775<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.9<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">52100<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">5160<\/td><td class=\"has-text-align-left\" data-align=\"left\">1525<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O1<\/td><td class=\"has-text-align-left\" data-align=\"left\">1475<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1095<\/td><td class=\"has-text-align-left\" data-align=\"left\">1475<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Fonte, <a href=\"https:\/\/aobosteel.com\/pt\/blog\/knife-steel-types\/\">resist\u00eancia \u00e0 corros\u00e3o de a\u00e7os para cutelaria<\/a>, Tabela 15.1 na fonte.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><em>A pontua\u00e7\u00e3o \u00e9 a equa\u00e7\u00e3o de resist\u00eancia \u00e0 corros\u00e3o que a fonte desenvolveu a partir de seus pr\u00f3prios ensaios de corros\u00e3o, cromo mais 1,6 vezes molibd\u00eanio mais 0,8 vezes tungst\u00eanio mais 6 vezes nitrog\u00eanio, aplicada \u00e0 liga que est\u00e1 em solu\u00e7\u00e3o na temperatura de austenitiza\u00e7\u00e3o listada para cada grau, com a contribui\u00e7\u00e3o de molibd\u00eanio, tungst\u00eanio e nitrog\u00eanio limitada. Presume-se que cada grau tenha recebido um revenimento a baixa temperatura. Uma pontua\u00e7\u00e3o de 11 ou superior \u00e9 a linha que a fonte usa para a palavra inoxid\u00e1vel. Apenas uma tabela de refer\u00eancia, n\u00e3o \u00e9 uma especifica\u00e7\u00e3o da Aobo Steel.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Como as fam\u00edlias de graus pontuam<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Os graus inoxid\u00e1veis martens\u00edticos ficam no topo da faixa que uma ferramentaria realmente compra. O 440A pontua 14,2, o 420 pontua 13,0 e o 440C pontua 12,5, ent\u00e3o os tr\u00eas graus que concentram a maior parte do trabalho em moldes, cutelaria e bombas est\u00e3o separados por menos de dois pontos, e <a href=\"https:\/\/aobosteel.com\/pt\/cpm-440v-vs-440c-wear-and-toughness\/\">o que os diferencia em servi\u00e7o \u00e9 a dureza e o carbono, e n\u00e3o a resist\u00eancia \u00e0 corros\u00e3o<\/a>. O 420HC pontua 12,5 no mesmo cromo que o 420, e o AEB-L e o 19C27 pontuam 11,7 e 11,5 com menor teor de carbono. Todos eles ultrapassam a linha em 11.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os a\u00e7os ferramenta para trabalho a frio e a\u00e7os r\u00e1pidos ficam no meio e abaixo. O D2 pontua 7,4 e o A2 pontua 5,3, ambos bem abaixo da linha, ent\u00e3o uma matriz de D2 enferruja em uma m\u00e1quina \u00famida mesmo carregando 12 por cento de cromo, porque a maior parte desse cromo est\u00e1 retida em carboneto e a matriz fica desprovida. O M2 e o M4 pontuam 6,9 e 6,6 com menos cromo e mais tungst\u00eanio e molibd\u00eanio, e o 52100, 5160, O1 e 1095 pontuam 1,0 ou menos com menos de 1 por cento de cromo. Nesta tabela esses quatro s\u00e3o a\u00e7o carbono com melhores maneiras.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os graus com nitrog\u00eanio e de metalurgia do p\u00f3 ocupam o topo da tabela. O Vanax e o LC200N pontuam 17,3 e 17,0 com cromo pr\u00f3ximo ao do 440A mais nitrog\u00eanio em solu\u00e7\u00e3o, e o M390 e o S110V pontuam 15,2 e 15,1 com cromo e molibd\u00eanio ao lado. Nenhum dos quatro \u00e9 estoque geral de ferramentaria, e o padr\u00e3o que eles estabelecem \u00e9 a parte \u00fatil. Nitrog\u00eanio e molibd\u00eanio em solu\u00e7\u00e3o elevam a pontua\u00e7\u00e3o mais r\u00e1pido do que o cromo, e \u00e9 por isso que um a\u00e7o para molde especificado para um trabalho \u00famido ou quimicamente agressivo \u00e9 selecionado pela an\u00e1lise completa e n\u00e3o apenas pelo n\u00famero de cromo. Dois graus com 12 a 13 por cento de cromo podem ficar quatro pontos distantes.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">O que move a pontua\u00e7\u00e3o em servi\u00e7o<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Tr\u00eas decis\u00f5es de tratamento t\u00e9rmico movem a pontua\u00e7\u00e3o mais do que a ficha do grau. A temperatura de austenitiza\u00e7\u00e3o define quanto cromo, molibd\u00eanio e tungst\u00eanio entram em solu\u00e7\u00e3o, e a temperatura listada para cada grau \u00e9 o ponto m\u00e9dio da faixa que uma ficha t\u00e9cnica fornece, ent\u00e3o endurecer na parte inferior da faixa deixa elemento de liga em carboneto e retorna uma pontua\u00e7\u00e3o mais baixa. O revenimento acima da faixa de endurecimento secund\u00e1rio precipita carboneto de cromo e retira cromo da solu\u00e7\u00e3o, e \u00e9 por isso que um revenimento em baixa temperatura \u00e9 presumido para cada grau na tabela. A austenita retida ret\u00e9m carbono e elemento de liga que de outra forma estariam na matriz, e ela reduz a pontua\u00e7\u00e3o at\u00e9 que um tratamento a frio ou um segundo revenimento a decomponha.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Read it as a <a href=\"https:\/\/aobosteel.com\/pt\/corrosion-testing-methods-steel\/\">classifica\u00e7\u00e3o da liga em solu\u00e7\u00e3o em vez de uma taxa de corros\u00e3o<\/a>. A pontua\u00e7\u00e3o indica quais graus vale a pena considerar para um trabalho \u00famido ou quimicamente agressivo e quais n\u00e3o, e a ficha t\u00e9cnica do grau ainda decide a dureza, a tenacidade e o acabamento de que a pe\u00e7a necessita.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>Tabela de resist\u00eancia \u00e0 corros\u00e3o, PDF para impress\u00e3o<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">Todos os 48 graus com seus teores de cromo, molibd\u00eanio, tungst\u00eanio e nitrog\u00eanio e a pontua\u00e7\u00e3o resultante, em um PDF com nossos dados de contato.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-Stainless-Steel-Corrosion-Resistance-Chart.pdf\">Baixar PDF, 470 KB<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<h2 class=\"wp-block-heading\">Dados de refer\u00eancia relacionados<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">As faixas de composi\u00e7\u00e3o para os graus inoxid\u00e1veis est\u00e3o na <a href=\"https:\/\/aobosteel.com\/pt\/stainless-steel-composition-chart\/\">tabela de composi\u00e7\u00e3o do a\u00e7o inoxid\u00e1vel<\/a>, e os dados de dureza, tra\u00e7\u00e3o e impacto para a mesma fam\u00edlia est\u00e3o na <a href=\"https:\/\/aobosteel.com\/pt\/martensitic-stainless-steel-properties-chart\/\">Tabela de propriedades do a\u00e7o inoxid\u00e1vel martens\u00edtico<\/a>. Os graus que mantemos em estoque e fornecemos s\u00e3o <a href=\"https:\/\/aobosteel.com\/pt\/420-stainless-steel\/\">a\u00e7o inoxid\u00e1vel 420<\/a> e <a href=\"https:\/\/aobosteel.com\/pt\/440c-stainless-steel\/\">a\u00e7o inoxid\u00e1vel 440C<\/a>. De onde vem a pontua\u00e7\u00e3o na microestrutura \u00e9 abordado na <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-carbide-types-and-hardness\/\">p\u00e1gina de tipos de carboneto de a\u00e7o ferramenta<\/a>, e a sele\u00e7\u00e3o de grau para um molde que v\u00ea umidade ou uma resina agressiva est\u00e1 na <a href=\"https:\/\/aobosteel.com\/pt\/blog\/plastic-injection-mold-steel-selection\/\">p\u00e1gina de sele\u00e7\u00e3o de a\u00e7o para moldes pl\u00e1sticos<\/a>. Os tratamentos superficiais que restauram a resist\u00eancia \u00e0 corros\u00e3o ap\u00f3s a usinagem est\u00e3o na <a href=\"https:\/\/aobosteel.com\/pt\/blog\/tool-steel-surface-treatment\/\">p\u00e1gina de tratamento superficial de a\u00e7o ferramenta<\/a>, e a mesma quest\u00e3o para os graus de trabalho a frio est\u00e1 na <a href=\"https:\/\/aobosteel.com\/pt\/d2-steel-vs-440c\/\">compara\u00e7\u00e3o D2 versus 440C<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Fonte: Knife Engineering, Steel, Heat Treating, and Geometry (Larrin Thomas).<\/p>","protected":false},"excerpt":{"rendered":"<p>Stainless Steel Corrosion Resistance Chart Corrosion resistance score for 48 stainless and tool steel grades, worked out from the chromium, molybdenum, tungsten and nitrogen left in solution. A reference summary of published practice and not an Aobo Steel specification. What the corrosion resistance score measures Rust resistance in a stainless steel comes from the chromium [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-20319","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Stainless Steel Corrosion Resistance Chart | 420, 440A, 440C<\/title>\n<meta name=\"description\" content=\"Corrosion resistance score for 48 stainless and tool steel grades, worked out from the chromium, molybdenum, tungsten and nitrogen left in solution.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/stainless-steel-corrosion-resistance-chart\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Stainless Steel Corrosion Resistance Chart\" \/>\n<meta property=\"og:description\" content=\"Corrosion resistance score for 48 stainless and tool steel grades, worked out from the chromium, molybdenum, tungsten and nitrogen left in solution.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/stainless-steel-corrosion-resistance-chart\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-11-09T00:08:01+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"6 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-corrosion-resistance-chart\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-corrosion-resistance-chart\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Stainless Steel Corrosion Resistance Chart\",\"datePublished\":\"2026-09-29T22:08:56+00:00\",\"dateModified\":\"2026-11-09T00:08:01+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-corrosion-resistance-chart\\\/\"},\"wordCount\":1144,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-corrosion-resistance-chart\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-corrosion-resistance-chart\\\/\",\"name\":\"Stainless Steel Corrosion Resistance Chart | 420, 440A, 440C\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-29T22:08:56+00:00\",\"dateModified\":\"2026-11-09T00:08:01+00:00\",\"description\":\"Corrosion resistance score for 48 stainless and tool steel grades, worked out from the chromium, molybdenum, tungsten and nitrogen left in solution.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-corrosion-resistance-chart\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-corrosion-resistance-chart\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-corrosion-resistance-chart\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Stainless Steel Corrosion Resistance Chart\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Tabela de resist\u00eancia \u00e0 corros\u00e3o do a\u00e7o inoxid\u00e1vel | 420, 440A, 440C","description":"Pontua\u00e7\u00e3o de resist\u00eancia \u00e0 corros\u00e3o de 48 a\u00e7os inoxid\u00e1veis e ferramenta, calculada a partir do cromo, molibd\u00eanio, tungst\u00eanio e nitrog\u00eanio em solu\u00e7\u00e3o.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/stainless-steel-corrosion-resistance-chart\/","og_locale":"pt_BR","og_type":"article","og_title":"Stainless Steel Corrosion Resistance Chart","og_description":"Corrosion resistance score for 48 stainless and tool steel grades, worked out from the chromium, molybdenum, tungsten and nitrogen left in solution.","og_url":"https:\/\/aobosteel.com\/pt\/stainless-steel-corrosion-resistance-chart\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-11-09T00:08:01+00:00","twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"6 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/stainless-steel-corrosion-resistance-chart\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/stainless-steel-corrosion-resistance-chart\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Stainless Steel Corrosion Resistance Chart","datePublished":"2026-09-29T22:08:56+00:00","dateModified":"2026-11-09T00:08:01+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/stainless-steel-corrosion-resistance-chart\/"},"wordCount":1144,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/stainless-steel-corrosion-resistance-chart\/","url":"https:\/\/aobosteel.com\/stainless-steel-corrosion-resistance-chart\/","name":"Tabela de resist\u00eancia \u00e0 corros\u00e3o do a\u00e7o inoxid\u00e1vel | 420, 440A, 440C","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-29T22:08:56+00:00","dateModified":"2026-11-09T00:08:01+00:00","description":"Pontua\u00e7\u00e3o de resist\u00eancia \u00e0 corros\u00e3o de 48 a\u00e7os inoxid\u00e1veis e ferramenta, calculada a partir do cromo, molibd\u00eanio, tungst\u00eanio e nitrog\u00eanio em solu\u00e7\u00e3o.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/stainless-steel-corrosion-resistance-chart\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/stainless-steel-corrosion-resistance-chart\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/stainless-steel-corrosion-resistance-chart\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Stainless Steel Corrosion Resistance Chart"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Stainless Steel Corrosion Resistance Chart Corrosion resistance score for 48 stainless and tool steel grades, worked out from the chromium, molybdenum, tungsten and nitrogen left in solution. A reference summary of published practice and not an Aobo Steel specification. What the corrosion resistance score measures Rust resistance in a stainless steel comes from the chromium&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Stainless Steel Corrosion Resistance Chart Corrosion resistance score for 48 stainless and tool steel grades, worked out from the chromium, molybdenum, tungsten and nitrogen left in solution. A reference summary of published practice and not an Aobo Steel specification. What the corrosion resistance score measures Rust resistance in a stainless steel comes from the chromium&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20319","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=20319"}],"version-history":[{"count":8,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20319\/revisions"}],"predecessor-version":[{"id":25128,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/20319\/revisions\/25128"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=20319"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}