{"id":19493,"date":"2026-09-22T00:41:20","date_gmt":"2026-09-21T16:41:20","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=19493"},"modified":"2026-10-15T23:48:59","modified_gmt":"2026-10-15T15:48:59","slug":"microalloyed-strip-steel-compositions","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/microalloyed-strip-steel-compositions\/","title":{"rendered":"Composi\u00e7\u00f5es e limite de escoamento de a\u00e7os de tira microligados"},"content":{"rendered":"<h1 class=\"wp-block-heading\">Composi\u00e7\u00f5es e limite de escoamento de a\u00e7os de tira microligados<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">Composi\u00e7\u00f5es em percentual em peso, condi\u00e7\u00f5es industriais de lamina\u00e7\u00e3o e limite de escoamento ap\u00f3s bobinamento para cinco a\u00e7os microligados comerciais para tiras a quente, desde uma base C-Mn com baixo ni\u00f3bio at\u00e9 graus NbTiV que atingem 599 a 638 MPa. As tabelas s\u00e3o um resumo de refer\u00eancia de um cap\u00edtulo publicado e n\u00e3o uma especifica\u00e7\u00e3o da Aobo Steel. A \u00faltima tabela divide o limite de escoamento medido na parte explicada pelo tamanho de gr\u00e3o e solu\u00e7\u00e3o s\u00f3lida e na parte contribu\u00edda por <a href=\"https:\/\/aobosteel.com\/pt\/microalloyed-steel-strengthening-mechanisms\/\">discord\u00e2ncias e precipita\u00e7\u00e3o de carbonitretos<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Composi\u00e7\u00f5es dos cinco a\u00e7os<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Todos os valores s\u00e3o em porcentagem de peso, conforme impresso. Um tra\u00e7o significa que a fonte n\u00e3o lista adi\u00e7\u00e3o desse elemento, e n.d. significa n\u00e3o determinado. A \u00faltima coluna \u00e9 a fra\u00e7\u00e3o volum\u00e9trica total m\u00e1xima dispon\u00edvel para precipita\u00e7\u00e3o de carbonitreto.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">A\u00e7o<\/th><th class=\"has-text-align-left\" data-align=\"left\">C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mn<\/th><th class=\"has-text-align-left\" data-align=\"left\">Si<\/th><th class=\"has-text-align-left\" data-align=\"left\">P<\/th><th class=\"has-text-align-left\" data-align=\"left\">S<\/th><th class=\"has-text-align-left\" data-align=\"left\">Al<\/th><th class=\"has-text-align-left\" data-align=\"left\">Nb<\/th><th class=\"has-text-align-left\" data-align=\"left\">Ti<\/th><th class=\"has-text-align-left\" data-align=\"left\">V<\/th><th class=\"has-text-align-left\" data-align=\"left\">N<\/th><th class=\"has-text-align-left\" data-align=\"left\">Vf<br>m\u00e1ximo<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Nb<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.07<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.68<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.01<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.012<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.009<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.009<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.00045<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTi-1<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.55<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">n.d.<\/td><td class=\"has-text-align-left\" data-align=\"left\">n.d.<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.02<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.006<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.00131<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTi-2<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.12<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.21<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.33<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.023<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.008<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.048<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.057<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.059<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.008<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.00166<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTi-3<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.11<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.54<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.28<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.026<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.007<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.01<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.11<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2013<\/td><td class=\"has-text-align-left\" data-align=\"left\">n.d.<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.00261<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTiV<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.14<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.38<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.018<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.007<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.07<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.04<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.03<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.008<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.00174<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Fonte, Alloy Steel, Properties and Use (E. Morales), cap\u00edtulo 3, Comments About the Strengthening Mechanisms in Commercial Microalloyed Steels and Reaction Kinetics on Tempering in Low-Alloy Steels, Tabela 5, p. 60.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>Composi\u00e7\u00f5es e limite de escoamento de a\u00e7os de tira microligados, PDF para impress\u00e3o<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">Duas p\u00e1ginas A4 com as cinco composi\u00e7\u00f5es de a\u00e7o em porcentagem de peso, as condi\u00e7\u00f5es de lamina\u00e7\u00e3o e o limite de escoamento ap\u00f3s bobinamento, e nossos dados de contato.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/09\/Aobo-Steel-Microalloyed-Strip-Steel-Compositions.pdf\">Baixar PDF, 430 KB<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<p class=\"wp-block-paragraph\">Condi\u00e7\u00f5es industriais de processamento e limite de escoamento ap\u00f3s bobinamento<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">As temperaturas de aquecimento, desbaste, acabamento e bobinamento s\u00e3o dadas em graus C, a espessura em mil\u00edmetros e o limite de escoamento em MPa. Todos os cinco a\u00e7os foram laminados em um laminador de tiras a quente industrial. A coluna de resfriamento est\u00e1 impressa como \u00b0C*min-1 na fonte e \u00e9 reproduzida sem altera\u00e7\u00e3o.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">A\u00e7o<\/th><th class=\"has-text-align-left\" data-align=\"left\">Encharcando<br>\u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Bruto<br>\u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Acabamento<br>\u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento<br>\u00b0C*min-1<\/th><th class=\"has-text-align-left\" data-align=\"left\">Bobinamento<br>\u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Grossura<br>mm<\/th><th class=\"has-text-align-left\" data-align=\"left\">L.E.<br>MPa<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Nb<\/td><td class=\"has-text-align-left\" data-align=\"left\">1150<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u22651080<\/td><td class=\"has-text-align-left\" data-align=\"left\">890<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">310<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTi-1<\/td><td class=\"has-text-align-left\" data-align=\"left\">1230<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u22651100<\/td><td class=\"has-text-align-left\" data-align=\"left\">870<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">630<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">332<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTi-2<\/td><td class=\"has-text-align-left\" data-align=\"left\">1150<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u22651070<\/td><td class=\"has-text-align-left\" data-align=\"left\">870<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">7<\/td><td class=\"has-text-align-left\" data-align=\"left\">534<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTi-3<\/td><td class=\"has-text-align-left\" data-align=\"left\">1225<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u22651100<\/td><td class=\"has-text-align-left\" data-align=\"left\">895<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">638<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTiV<\/td><td class=\"has-text-align-left\" data-align=\"left\">1225<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u22651100<\/td><td class=\"has-text-align-left\" data-align=\"left\">895<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><td class=\"has-text-align-left\" data-align=\"left\">670<\/td><td class=\"has-text-align-left\" data-align=\"left\">3<\/td><td class=\"has-text-align-left\" data-align=\"left\">599<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Fonte, Alloy Steel, Properties and Use (E. Morales), cap\u00edtulo 3, Comments About the Strengthening Mechanisms in Commercial Microalloyed Steels and Reaction Kinetics on Tempering in Low-Alloy Steels, Tabela 6, p. 60.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">De onde vem o limite de escoamento<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O limite de escoamento base \u00e9 calculado a partir do tamanho de gr\u00e3o ferr\u00edtico, mangan\u00eas, sil\u00edcio e nitrog\u00eanio livre em solu\u00e7\u00e3o. A \u00faltima coluna \u00e9 o endurecimento adicional por discord\u00e2ncias e precipita\u00e7\u00e3o, obtido subtraindo o valor base calculado do limite de escoamento medido. A fonte imprime o cabe\u00e7alho da \u00faltima coluna como \u0394\u03c3( MPa, reproduzido aqui como \u0394\u03c3 (MPa).<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">A\u00e7o<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tamanho do gr\u00e3o<br>(\u00b5m)<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u03c3<br>(MPa)<\/th><th class=\"has-text-align-left\" data-align=\"left\">\u0394\u03c3<br>(MPa)<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Nb<\/td><td class=\"has-text-align-left\" data-align=\"left\">10.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">252<\/td><td class=\"has-text-align-left\" data-align=\"left\">58<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTi-1<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">254<\/td><td class=\"has-text-align-left\" data-align=\"left\">78<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTi-2<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.0<\/td><td class=\"has-text-align-left\" data-align=\"left\">367<\/td><td class=\"has-text-align-left\" data-align=\"left\">167<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTi-3<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">393<\/td><td class=\"has-text-align-left\" data-align=\"left\">245<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">NbTiV<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.3<\/td><td class=\"has-text-align-left\" data-align=\"left\">421<\/td><td class=\"has-text-align-left\" data-align=\"left\">178<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Fonte, Alloy Steel, Properties and Use (E. Morales), cap\u00edtulo 3, Comments About the Strengthening Mechanisms in Commercial Microalloyed Steels and Reaction Kinetics on Tempering in Low-Alloy Steels, Tabela 7, p. 61.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Carbono e mangan\u00eas definem o n\u00edvel de resist\u00eancia. O a\u00e7o Nb com 0,07 % C e 0,68 % Mn atingiu 310 MPa ap\u00f3s bobinamento, enquanto o NbTi-2 com 0,12 % C e 1,21 % Mn atingiu 534 MPa. Os tr\u00eas a\u00e7os de maior resist\u00eancia cont\u00eam ni\u00f3bio com tit\u00e2nio, e o NbTiV adiciona tamb\u00e9m van\u00e1dio. Para as composi\u00e7\u00f5es dos graus de a\u00e7o liga que fornecemos como barra, consulte o <a href=\"https:\/\/aobosteel.com\/pt\/alloy-steel-composition-chart\/\">Tabela de composi\u00e7\u00e3o de a\u00e7o liga<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os tr\u00eas a\u00e7os de maior resist\u00eancia tamb\u00e9m sa\u00edram do laminador mais finos, com 3 a 8 mm contra 10 mm dos dois de menor resist\u00eancia, e seu tamanho de gr\u00e3o ferr\u00edtico caiu para 3,3 a 5,0 \u00b5m contra cerca de 10 \u00b5m. O refino de gr\u00e3o \u00e9 a maior parte desse ganho. O endurecimento adicional por discord\u00e2ncias e precipita\u00e7\u00e3o varia de 58 MPa no a\u00e7o Nb a 245 MPa no NbTi-3.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os nomes dos a\u00e7os Nb, NbTi-1, NbTi-2, NbTi-3 e NbTiV s\u00e3o os identificadores usados no cap\u00edtulo da fonte, n\u00e3o designa\u00e7\u00f5es comerciais de grau. Os n\u00fameros acima s\u00e3o os valores impressos nesse cap\u00edtulo, n\u00e3o uma especifica\u00e7\u00e3o de compra. A composi\u00e7\u00e3o dos graus de a\u00e7o carbono que fornecemos est\u00e1 no <a href=\"https:\/\/aobosteel.com\/pt\/carbon-steel-composition-chart\/\">Tabela de composi\u00e7\u00e3o do a\u00e7o carbono<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os dados de composi\u00e7\u00e3o e propriedades s\u00e3o apenas para refer\u00eancia geral. Os valores reais variam conforme a norma, o laminador e o n\u00famero de corrida. Confirme com o certificado de ensaio do material (MTC) ou entre em contato com a Aobo Steel.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Dados de refer\u00eancia compilados de Alloy Steel, Properties and Use (E. Morales), cap\u00edtulo 3, Comments About the Strengthening Mechanisms in Commercial Microalloyed Steels and Reaction Kinetics on Tempering in Low-Alloy Steels.<\/p>","protected":false},"excerpt":{"rendered":"<p>Microalloyed Strip Steel Compositions and Yield Strength Compositions in weight percent, industrial rolling conditions and yield strength after coiling for five commercial microalloyed hot strip steels, from a low niobium C-Mn baseline to NbTiV grades that reach 599 to 638 MPa. The tables are a reference summary of a published chapter and not an Aobo [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-19493","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Microalloyed Steel Compositions | Nb, NbTi, NbTiV Grades<\/title>\n<meta name=\"description\" content=\"Compositions in weight percent, rolling conditions and yield strength after coiling for five commercial microalloyed hot strip steels, from a C-Mn Nb baseline to NbTiV grades.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/microalloyed-strip-steel-compositions\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Microalloyed Strip Steel Compositions and Yield Strength\" \/>\n<meta property=\"og:description\" content=\"Compositions in weight percent, rolling conditions and yield strength after coiling for five commercial microalloyed hot strip steels, from a C-Mn Nb baseline to NbTiV grades.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/microalloyed-strip-steel-compositions\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T15:48:59+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"3 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/microalloyed-strip-steel-compositions\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/microalloyed-strip-steel-compositions\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Microalloyed Strip Steel Compositions and Yield Strength\",\"datePublished\":\"2026-09-21T16:41:20+00:00\",\"dateModified\":\"2026-10-15T15:48:59+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/microalloyed-strip-steel-compositions\\\/\"},\"wordCount\":653,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/microalloyed-strip-steel-compositions\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/microalloyed-strip-steel-compositions\\\/\",\"name\":\"Microalloyed Steel Compositions | Nb, NbTi, NbTiV Grades\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-09-21T16:41:20+00:00\",\"dateModified\":\"2026-10-15T15:48:59+00:00\",\"description\":\"Compositions in weight percent, rolling conditions and yield strength after coiling for five commercial microalloyed hot strip steels, from a C-Mn Nb baseline to NbTiV grades.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/microalloyed-strip-steel-compositions\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/microalloyed-strip-steel-compositions\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/microalloyed-strip-steel-compositions\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Microalloyed Strip Steel Compositions and Yield Strength\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Composi\u00e7\u00f5es de a\u00e7o microligado | Graus Nb, NbTi, NbTiV","description":"Composi\u00e7\u00f5es em porcentagem de peso, condi\u00e7\u00f5es de lamina\u00e7\u00e3o e limite de escoamento ap\u00f3s bobinamento para cinco a\u00e7os de tira a quente microligados comerciais, de uma base C-Mn Nb a graus NbTiV.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/microalloyed-strip-steel-compositions\/","og_locale":"pt_BR","og_type":"article","og_title":"Microalloyed Strip Steel Compositions and Yield Strength","og_description":"Compositions in weight percent, rolling conditions and yield strength after coiling for five commercial microalloyed hot strip steels, from a C-Mn Nb baseline to NbTiV grades.","og_url":"https:\/\/aobosteel.com\/pt\/microalloyed-strip-steel-compositions\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T15:48:59+00:00","twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"3 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/microalloyed-strip-steel-compositions\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/microalloyed-strip-steel-compositions\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Microalloyed Strip Steel Compositions and Yield Strength","datePublished":"2026-09-21T16:41:20+00:00","dateModified":"2026-10-15T15:48:59+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/microalloyed-strip-steel-compositions\/"},"wordCount":653,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/microalloyed-strip-steel-compositions\/","url":"https:\/\/aobosteel.com\/microalloyed-strip-steel-compositions\/","name":"Composi\u00e7\u00f5es de a\u00e7o microligado | Graus Nb, NbTi, NbTiV","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-09-21T16:41:20+00:00","dateModified":"2026-10-15T15:48:59+00:00","description":"Composi\u00e7\u00f5es em porcentagem de peso, condi\u00e7\u00f5es de lamina\u00e7\u00e3o e limite de escoamento ap\u00f3s bobinamento para cinco a\u00e7os de tira a quente microligados comerciais, de uma base C-Mn Nb a graus NbTiV.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/microalloyed-strip-steel-compositions\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/microalloyed-strip-steel-compositions\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/microalloyed-strip-steel-compositions\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Microalloyed Strip Steel Compositions and Yield Strength"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Microalloyed Strip Steel Compositions and Yield Strength Compositions in weight percent, industrial rolling conditions and yield strength after coiling for five commercial microalloyed hot strip steels, from a low niobium C-Mn baseline to NbTiV grades that reach 599 to 638 MPa. The tables are a reference summary of a published chapter and not an Aobo&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Microalloyed Strip Steel Compositions and Yield Strength Compositions in weight percent, industrial rolling conditions and yield strength after coiling for five commercial microalloyed hot strip steels, from a low niobium C-Mn baseline to NbTiV grades that reach 599 to 638 MPa. The tables are a reference summary of a published chapter and not an Aobo&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/19493","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=19493"}],"version-history":[{"count":6,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/19493\/revisions"}],"predecessor-version":[{"id":22450,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/19493\/revisions\/22450"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=19493"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}