{"id":17163,"date":"2026-07-31T09:28:48","date_gmt":"2026-07-31T01:28:48","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=17163"},"modified":"2026-10-21T20:57:22","modified_gmt":"2026-10-21T12:57:22","slug":"tool-steel-annealing-normalizing-temperature-chart","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/pt\/tool-steel-annealing-normalizing-temperature-chart\/","title":{"rendered":"Tabela de temperaturas de recozimento e normaliza\u00e7\u00e3o de a\u00e7o ferramenta"},"content":{"rendered":"<h1 class=\"wp-block-heading\">Normaliza\u00e7\u00e3o, recozimento, t\u00eampera e revenimento de a\u00e7os para ferramentas<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">Refer\u00eancia completa para temperaturas de tratamento t\u00e9rmico de todos os principais graus de a\u00e7o ferramenta, com valores em \u00b0C e \u00b0F. O cronograma de t\u00eampera e revenimento tamb\u00e9m \u00e9 publicado como tabela independente no <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-hardening-tempering-chart\/\">gr\u00e1fico de temperatura de endurecimento e revenimento<\/a>, e a sequ\u00eancia geral do processo \u00e9 abordada no <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-heat-treatment-guide\/\">guia de tratamento t\u00e9rmico de a\u00e7o ferramenta<\/a>.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-06220d26 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f2f5f9;padding-top:12px;padding-right:18px;padding-bottom:12px;padding-left:18px\">\n<p class=\"wp-block-paragraph\"><strong>O<\/strong> = T\u00eampera em \u00f3leo &middot; <strong>A<\/strong> = Resfriamento ao ar &middot; <strong>S<\/strong> = T\u00eampera em banho de sal &middot; <strong>W<\/strong> = T\u00eampera em \u00e1gua &middot; <strong>B<\/strong> = Resfriamento com salmoura<\/p>\n<\/div>\n\n\n\n<h2 class=\"wp-block-heading\">Normaliza\u00e7\u00e3o e Recozimento<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\"><a href=\"https:\/\/aobosteel.com\/pt\/high-speed-steels\/\">A\u00e7os r\u00e1pidos ao molibd\u00eanio<\/a><\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/m1-tool-steel-heat-treatment\/\">M1<\/a>, M10<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">815-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">207-235<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/m2-tool-steel\/\">M2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">212-241<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M3, M4<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">223-255<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M7<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">815-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">217-255<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M30, M33, M34, <a href=\"https:\/\/aobosteel.com\/pt\/m35-tool-steel\/\">M35<\/a>, M36, M41, <a href=\"https:\/\/aobosteel.com\/pt\/m42-tool-steel\/\">M42<\/a>, M46, M47<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">235-269<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M43<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">248-269<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M44<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">248-293<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M48<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">285-311<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M62<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">262-285<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os r\u00e1pidos ao tungst\u00eanio<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">T1<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">217-255<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T2<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">223-255<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T4<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">229-269<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T5<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">235-277<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T6<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">248-293<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T8<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">229-255<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T15<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">241-277<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os r\u00e1pidos intermedi\u00e1rios<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">M50<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">830-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1525-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">197-235<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M52<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">830-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1525-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">197-235<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\"><a href=\"https:\/\/aobosteel.com\/pt\/hot-work-tool-steels\/\">A\u00e7os para trabalho a quente ao cromo<\/a><\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/h10-tool-steel\/\">H10<\/a>, <a href=\"https:\/\/aobosteel.com\/pt\/h11-tool-steel\/\">H11<\/a>, H12, <a href=\"https:\/\/aobosteel.com\/pt\/h13-tool-steel\/\">H13<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">845-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">192-229<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H14<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">207-235<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H19<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">207-241<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os para trabalho a quente ao tungst\u00eanio<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/h21-tool-steel\/\">H21<\/a>, H22, H25<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">207-235<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H23<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">212-255<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H24, H26<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">217-241<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os para trabalho a quente ao molibd\u00eanio<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">H41, H43<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">815-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">207-235<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H42<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">845-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">207-235<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\"><a href=\"https:\/\/aobosteel.com\/pt\/d-series-tool-steels\/\">A\u00e7os para trabalho a frio com alto teor de carbono e cromo<\/a><\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/d2-tool-steel\/\">D2<\/a>, <a href=\"https:\/\/aobosteel.com\/pt\/d3-tool-steel\/\">D3<\/a>, D4<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">217-255<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D5<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">223-255<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D7<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">235-262<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\"><a href=\"https:\/\/aobosteel.com\/pt\/air-hardening-tool-steel\/\">A\u00e7os para Trabalho a Frio de M\u00e9dia Liga, Endurec\u00edveis ao Ar<\/a><\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/a2-tool-steel\/\">A2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">845-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">201-229<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A3<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">845-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">207-229<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A4<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">740-760<\/td><td class=\"has-text-align-left\" data-align=\"left\">1360-1400<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">200-241<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-745<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1375<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">217-248<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A7<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">235-262<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A8<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">845-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">192-223<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/a9-tool-steel-heat-treatment\/\">A9<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">845-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">212-248<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A10<\/td><td class=\"has-text-align-left\" data-align=\"left\">790 \/ 1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">765-795<\/td><td class=\"has-text-align-left\" data-align=\"left\">1410-1460<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">235-269<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\"><a href=\"https:\/\/aobosteel.com\/pt\/oil-hardening-tool-steel\/\">A\u00e7os para trabalho a frio com t\u00eampera em \u00f3leo<\/a><\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/o1-tool-steel\/\">O1<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">870 \/ 1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">760-790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">183-212<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/o2-tool-steel\/\">O2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">845 \/ 1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">770-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1375-1425<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">183-212<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O6<\/td><td class=\"has-text-align-left\" data-align=\"left\">870 \/ 1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">765-790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1410-1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">11<\/td><td class=\"has-text-align-left\" data-align=\"left\">20<\/td><td class=\"has-text-align-left\" data-align=\"left\">183-217<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O7<\/td><td class=\"has-text-align-left\" data-align=\"left\">900 \/ 1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">790-815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">192-217<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\"><a href=\"https:\/\/aobosteel.com\/pt\/s-series-tool-steel\/\">A\u00e7os resistentes ao choque<\/a><\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/s1-tool-steel\/\">S1<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">790-815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">183-229 (c)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S2<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">760-790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">192-217<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S5<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">775-800<\/td><td class=\"has-text-align-left\" data-align=\"left\">1425-1475<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">192-229<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/s7-tool-steel\/\">S7<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">815-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">187-223<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\"><a href=\"https:\/\/aobosteel.com\/pt\/plastic-mold-steels\/\">A\u00e7os para moldes<\/a><\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">P2<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o necess\u00e1rio<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">103-123<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P3<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o necess\u00e1rio<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">109-137<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P4<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o normalizar<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">14<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">116-128<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P5<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o necess\u00e1rio<\/td><td class=\"has-text-align-left\" data-align=\"left\">845-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">105-116<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P6<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o necess\u00e1rio<\/td><td class=\"has-text-align-left\" data-align=\"left\">845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">183-217<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/p20-tool-steel\/\">P20<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">900 \/ 1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">760-790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">149-179<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P21<\/td><td class=\"has-text-align-left\" data-align=\"left\">900 \/ 1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o recozer<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o recozer<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os especiais de baixa liga<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">L2<\/td><td class=\"has-text-align-left\" data-align=\"left\">871-900 \/ 1600-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">760-790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">163-197<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L3<\/td><td class=\"has-text-align-left\" data-align=\"left\">900 \/ 1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">790-815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">174-201<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/l6-tool-steel\/\">L6<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">870 \/ 1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">760-790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">183-212<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os Especiais Carbono-Tungst\u00eanio<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">F1<\/td><td class=\"has-text-align-left\" data-align=\"left\">900 \/ 1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">760-800<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1475<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">183-207<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">F2<\/td><td class=\"has-text-align-left\" data-align=\"left\">900 \/ 1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">790-815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">207-235<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os Endurec\u00edveis em \u00c1gua<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Normaliza\u00e7\u00e3o (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Recozimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0C\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Resfriamento m\u00e1x. \u00b0F\/h<\/th><th class=\"has-text-align-left\" data-align=\"left\">Dureza, HB<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">W1, W2<\/td><td class=\"has-text-align-left\" data-align=\"left\">790-925 (d)<\/td><td class=\"has-text-align-left\" data-align=\"left\">740-790 (e)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1360-1450 (e)<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">156-201<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">W5<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-925 \/ 1600-1700<\/td><td class=\"has-text-align-left\" data-align=\"left\">760-790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">22<\/td><td class=\"has-text-align-left\" data-align=\"left\">40<\/td><td class=\"has-text-align-left\" data-align=\"left\">163-201<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">Notas e refer\u00eancias<\/h3>\n\n\n\n<ol class=\"wp-block-list\">\n<li>(a) O tempo de perman\u00eancia na temperatura varia de 15 min para se\u00e7\u00f5es pequenas a 1 h para tamanhos grandes. O resfriamento \u00e9 feito ao ar calmo. A normaliza\u00e7\u00e3o n\u00e3o deve ser confundida com <a href=\"https:\/\/aobosteel.com\/pt\/high-speed-steel-softening-chart\/\">recozimento a baixa temperatura<\/a>.<\/li>\n\n<li>(b) O limite superior das faixas deve ser usado para se\u00e7\u00f5es grandes, e o limite inferior para se\u00e7\u00f5es menores. O tempo de perman\u00eancia na temperatura varia de 1 h para se\u00e7\u00f5es leves a 4 h para se\u00e7\u00f5es pesadas e grandes cargas de forno de a\u00e7o de alta liga.<\/li>\n\n<li>(c) Para o tipo 0,25 Si, 183 a 207 HB; para o tipo 1,00 Si, 207 a 229 HB.<\/li>\n\n<li>(d) A temperatura varia com o teor de carbono: 0,60\u20130,75 C, 815 \u00b0C (1500 \u00b0F); 0,75\u20130,90 C, 790 \u00b0C (1450 \u00b0F); 0,90\u20131,10 C, 870 \u00b0C (1600 \u00b0F); 1,10\u20131,40 C, 870\u2013925 \u00b0C (1600\u20131700 \u00b0F).<\/li>\n\n<li>(e) A temperatura varia com o teor de carbono: 0,60\u20130,90 C, 740\u2013790 \u00b0C (1360\u20131450 \u00b0F); 0,90\u20131,40 C, 760\u2013790 \u00b0C (1400\u20131450 \u00b0F).<\/li>\n<\/ol>\n\n\n\n<h2 class=\"wp-block-heading\">T\u00eampera e revenimento<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os r\u00e1pidos ao molibd\u00eanio<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">M1, M7, M10<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1175-1220 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2150-2225 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-595 (c)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1100 (c)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/m2-tool-steel-heat-treatment\/\">M2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190-1230 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2175-2250 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-595 (c)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1100 (c)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M3, M4, M30, M33, M34, M35<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1205-1230 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2200-2250 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-595 (c)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1100 (c)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M36<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1220-1245 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2225-2275 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-595 (c)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1100 (c)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M41<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190-1215 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2175-2220 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-595 (d)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1100 (d)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M42<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190-1210 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2175-2210 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">510-595 (d)<\/td><td class=\"has-text-align-left\" data-align=\"left\">950-1100 (d)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M43<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190-1215 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2175-2220 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">510-595 (d)<\/td><td class=\"has-text-align-left\" data-align=\"left\">950-1100 (d)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M44<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200-1225 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2190-2240 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-625 (d)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1160 (d)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M46<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1190-1220 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2175-2225 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">525-565 (d)<\/td><td class=\"has-text-align-left\" data-align=\"left\">975-1050 (d)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M47<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1175-1200 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2150-2200 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">525-595 (d)<\/td><td class=\"has-text-align-left\" data-align=\"left\">975-1100 (d)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M48<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1175-1200 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2150-2200 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-595 (d)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1100 (d)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M62<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1175-1200 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2150-2200 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-595 (d)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1100 (d)<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os r\u00e1pidos ao tungst\u00eanio<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">T1, T2, T4, T8<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">1260-1300 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2300-2375 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-595 (c)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1100 (c)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T5, T6<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">1275-1300 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2325-2375 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-595 (c)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1100 (c)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T15<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">1205-1260 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2200-2300 (b)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-650 (d)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1200 (d)<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os r\u00e1pidos intermedi\u00e1rios<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">M50<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1095-1120<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000-2050<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">525-595<\/td><td class=\"has-text-align-left\" data-align=\"left\">975-1100<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M52<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1120-1175<\/td><td class=\"has-text-align-left\" data-align=\"left\">2050-2150<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">525-595<\/td><td class=\"has-text-align-left\" data-align=\"left\">975-1100<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os para trabalho a quente ao cromo<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/h10-tool-steel-heat-treatment-guide\/\">H10<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Moderadamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">1010-1040<\/td><td class=\"has-text-align-left\" data-align=\"left\">1850-1900<\/td><td class=\"has-text-align-left\" data-align=\"left\">15-40 (e)<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1200<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/h11-tool-steel-heat-treatment\/\">H11<\/a>, H12<\/td><td class=\"has-text-align-left\" data-align=\"left\">Moderadamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">995-1025<\/td><td class=\"has-text-align-left\" data-align=\"left\">1825-1875<\/td><td class=\"has-text-align-left\" data-align=\"left\">15-40 (e)<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1200<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/h13-steel-heat-treatment\/\">H13<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Moderadamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">995-1040<\/td><td class=\"has-text-align-left\" data-align=\"left\">1825-1900<\/td><td class=\"has-text-align-left\" data-align=\"left\">15-40 (e)<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1200<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H14<\/td><td class=\"has-text-align-left\" data-align=\"left\">Moderadamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">1010-1065<\/td><td class=\"has-text-align-left\" data-align=\"left\">1850-1950<\/td><td class=\"has-text-align-left\" data-align=\"left\">15-40 (e)<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1200<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H19<\/td><td class=\"has-text-align-left\" data-align=\"left\">Moderadamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">1095-1205<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000-2200<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">A ou O<\/td><td class=\"has-text-align-left\" data-align=\"left\">540-705<\/td><td class=\"has-text-align-left\" data-align=\"left\">1000-1300<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os para trabalho a quente ao tungst\u00eanio<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">H21, H22<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">1095-1205<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000-2200<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">A ou O<\/td><td class=\"has-text-align-left\" data-align=\"left\">595-675<\/td><td class=\"has-text-align-left\" data-align=\"left\">1100-1250<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H23<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1205-1260<\/td><td class=\"has-text-align-left\" data-align=\"left\">2200-2300<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">650-815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200-1500<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H24<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">1095-1230<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000-2250<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">565-650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1050-1200<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H25<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">1150-1260<\/td><td class=\"has-text-align-left\" data-align=\"left\">2100-2300<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">A ou O<\/td><td class=\"has-text-align-left\" data-align=\"left\">565-675<\/td><td class=\"has-text-align-left\" data-align=\"left\">1050-1250<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H26<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">1175-1260<\/td><td class=\"has-text-align-left\" data-align=\"left\">2150-2300<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">565-675<\/td><td class=\"has-text-align-left\" data-align=\"left\">1050-1250<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os para trabalho a quente ao molibd\u00eanio<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">H41, H43<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1095-1190<\/td><td class=\"has-text-align-left\" data-align=\"left\">2000-2175<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">565-650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1050-1200<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H42<\/td><td class=\"has-text-align-left\" data-align=\"left\">Rapidamente a partir do pr\u00e9-aquecimento<\/td><td class=\"has-text-align-left\" data-align=\"left\">730-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1350-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">1120-1220<\/td><td class=\"has-text-align-left\" data-align=\"left\">2050-2225<\/td><td class=\"has-text-align-left\" data-align=\"left\">2-5<\/td><td class=\"has-text-align-left\" data-align=\"left\">O, A ou S<\/td><td class=\"has-text-align-left\" data-align=\"left\">565-650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1050-1200<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os para trabalho a frio com alto teor de carbono e cromo<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">D1, D5<\/td><td class=\"has-text-align-left\" data-align=\"left\">Muito lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">980-1025<\/td><td class=\"has-text-align-left\" data-align=\"left\">1800-1875<\/td><td class=\"has-text-align-left\" data-align=\"left\">15-45<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">205-540<\/td><td class=\"has-text-align-left\" data-align=\"left\">400-1000<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/d3-tool-steel-heat-treatment\/\">D3<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Muito lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">925-980<\/td><td class=\"has-text-align-left\" data-align=\"left\">1700-1800<\/td><td class=\"has-text-align-left\" data-align=\"left\">15-45<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">205-540<\/td><td class=\"has-text-align-left\" data-align=\"left\">400-1000<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D4<\/td><td class=\"has-text-align-left\" data-align=\"left\">Muito lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">970-1010<\/td><td class=\"has-text-align-left\" data-align=\"left\">1775-1850<\/td><td class=\"has-text-align-left\" data-align=\"left\">15-45<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">205-540<\/td><td class=\"has-text-align-left\" data-align=\"left\">400-1000<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D7<\/td><td class=\"has-text-align-left\" data-align=\"left\">Muito lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">1010-1065<\/td><td class=\"has-text-align-left\" data-align=\"left\">1850-1950<\/td><td class=\"has-text-align-left\" data-align=\"left\">30-60<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">150-540<\/td><td class=\"has-text-align-left\" data-align=\"left\">300-1000<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os para Trabalho a Frio de M\u00e9dia Liga, Endurec\u00edveis ao Ar<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/a2-tool-steel-heat-treatment-guide\/\">A2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">925-980<\/td><td class=\"has-text-align-left\" data-align=\"left\">1700-1800<\/td><td class=\"has-text-align-left\" data-align=\"left\">20-45<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-540<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-1000<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A3<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">955-980<\/td><td class=\"has-text-align-left\" data-align=\"left\">1750-1800<\/td><td class=\"has-text-align-left\" data-align=\"left\">25-60<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-540<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-1000<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A4<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">675<\/td><td class=\"has-text-align-left\" data-align=\"left\">1250<\/td><td class=\"has-text-align-left\" data-align=\"left\">815-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">20-45<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-425<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-800<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A6<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200<\/td><td class=\"has-text-align-left\" data-align=\"left\">830-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1525-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">20-45<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">150-425<\/td><td class=\"has-text-align-left\" data-align=\"left\">300-800<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A7<\/td><td class=\"has-text-align-left\" data-align=\"left\">Muito lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">955-980<\/td><td class=\"has-text-align-left\" data-align=\"left\">1750-1800<\/td><td class=\"has-text-align-left\" data-align=\"left\">30-60<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">150-540<\/td><td class=\"has-text-align-left\" data-align=\"left\">300-1000<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A8<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">980-1010<\/td><td class=\"has-text-align-left\" data-align=\"left\">1800-1850<\/td><td class=\"has-text-align-left\" data-align=\"left\">20-45<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-595<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-1100<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A9<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">790<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450<\/td><td class=\"has-text-align-left\" data-align=\"left\">980-1025<\/td><td class=\"has-text-align-left\" data-align=\"left\">1800-1875<\/td><td class=\"has-text-align-left\" data-align=\"left\">20-45<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">510-620<\/td><td class=\"has-text-align-left\" data-align=\"left\">950-1150<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/a10-tool-steel-heat-treatment\/\">A10<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200<\/td><td class=\"has-text-align-left\" data-align=\"left\">790-815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">30-60<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-425<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-800<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os para trabalho a frio com t\u00eampera em \u00f3leo<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/o1-tool-steel-heat-treatment\/\">O1<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200<\/td><td class=\"has-text-align-left\" data-align=\"left\">790-815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">10-30<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-260<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-500<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/o2-tool-steel-heat-treatment\/\">O2<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200<\/td><td class=\"has-text-align-left\" data-align=\"left\">760-800<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1475<\/td><td class=\"has-text-align-left\" data-align=\"left\">5-20<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-260<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-500<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O6<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">790-815<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1500<\/td><td class=\"has-text-align-left\" data-align=\"left\">10-30<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-315<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-600<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O7<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200<\/td><td class=\"has-text-align-left\" data-align=\"left\">W: 790-830 \/ O: 845-885<\/td><td class=\"has-text-align-left\" data-align=\"left\">W: 1450-1525 \/ O: 1550-1625<\/td><td class=\"has-text-align-left\" data-align=\"left\">10-30<\/td><td class=\"has-text-align-left\" data-align=\"left\">O ou W<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-290<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-550<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os resistentes ao choque<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/s1-tool-steel-heat-treatment-guide\/\">S1<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">900-955<\/td><td class=\"has-text-align-left\" data-align=\"left\">1650-1750<\/td><td class=\"has-text-align-left\" data-align=\"left\">15-45<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">205-650<\/td><td class=\"has-text-align-left\" data-align=\"left\">400-1200<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S2<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">650 (f)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200 (f)<\/td><td class=\"has-text-align-left\" data-align=\"left\">845-900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1550-1650<\/td><td class=\"has-text-align-left\" data-align=\"left\">5-20<\/td><td class=\"has-text-align-left\" data-align=\"left\">B ou W<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-425<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-800<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S5<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">760<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-925<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1700<\/td><td class=\"has-text-align-left\" data-align=\"left\">5-20<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-425<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-800<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/s7-tool-steel-heat-treatment\/\">S7<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">650-705<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200-1300<\/td><td class=\"has-text-align-left\" data-align=\"left\">925-955<\/td><td class=\"has-text-align-left\" data-align=\"left\">1700-1750<\/td><td class=\"has-text-align-left\" data-align=\"left\">15-45<\/td><td class=\"has-text-align-left\" data-align=\"left\">A ou O<\/td><td class=\"has-text-align-left\" data-align=\"left\">205-260<\/td><td class=\"has-text-align-left\" data-align=\"left\">400-500<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os para moldes<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">P2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">900-925 (g) \/ 830-845 (h)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1650-1750 (g) \/ 1525-1550 (h)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-260<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-500<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P3<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">900-925 (g) \/ 800-830 (h)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1650-1700 (g) \/ 1475-1525 (h)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-260<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-500<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">970-995 (g) \/ 970-995 (h)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1775-1825 (g) \/ 1775-1825 (h)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">A<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-480<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-900<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P5<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">900-925 (g) \/ 845-870 (h)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1650-1700 (g) \/ 1550-1600 (h)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">O ou W<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-260<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-500<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P6<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">900-925 (g) \/ 790-815 (h)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1650-1700 (g) \/ 1450-1500 (h)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">A ou O<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-450<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P20<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">870-900 (h) \/ 815-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1600-1650 (h) \/ 1500-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">480-595 (i)<\/td><td class=\"has-text-align-left\" data-align=\"left\">900-1100 (i)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">P21 (j)<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">N\u00e3o pr\u00e9-aquecer<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">705-730<\/td><td class=\"has-text-align-left\" data-align=\"left\">1300-1350<\/td><td class=\"has-text-align-left\" data-align=\"left\">60-180<\/td><td class=\"has-text-align-left\" data-align=\"left\">A ou O<\/td><td class=\"has-text-align-left\" data-align=\"left\">510-550<\/td><td class=\"has-text-align-left\" data-align=\"left\">950-1025<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os especiais de baixa liga<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">L2<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">W: 790-845 \/ O: 845-925<\/td><td class=\"has-text-align-left\" data-align=\"left\">W: 1450-1550 \/ O: 1550-1700<\/td><td class=\"has-text-align-left\" data-align=\"left\">10-30<\/td><td class=\"has-text-align-left\" data-align=\"left\">O ou W<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-540<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-1000<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L3<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">W: 775-815 \/ O: 815-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">W: 1425-1500 \/ O: 1500-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">10-30<\/td><td class=\"has-text-align-left\" data-align=\"left\">O ou W<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-315<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-600<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\"><a href=\"https:\/\/aobosteel.com\/pt\/l6-tool-steel-heat-treatment\/\">L6<\/a><\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u2014<\/td><td class=\"has-text-align-left\" data-align=\"left\">790-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">10-30<\/td><td class=\"has-text-align-left\" data-align=\"left\">O<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-540<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-1000<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os Especiais Carbono-Tungst\u00eanio<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">F1, F2<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200<\/td><td class=\"has-text-align-left\" data-align=\"left\">790-870<\/td><td class=\"has-text-align-left\" data-align=\"left\">1450-1600<\/td><td class=\"has-text-align-left\" data-align=\"left\">15<\/td><td class=\"has-text-align-left\" data-align=\"left\">W ou B<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-260<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-500<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">A\u00e7os Endurec\u00edveis em \u00c1gua<\/h3>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Tipo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Taxa de aquecimento<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Pr\u00e9-aquecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Endurecimento \u00b0F<\/th><th class=\"has-text-align-left\" data-align=\"left\">Tempo, min<\/th><th class=\"has-text-align-left\" data-align=\"left\">T\u00eampera (a)<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Revenimento \u00b0F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">W1, W2, W3<\/td><td class=\"has-text-align-left\" data-align=\"left\">Lentamente<\/td><td class=\"has-text-align-left\" data-align=\"left\">565-650 (k)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1050-1200 (k)<\/td><td class=\"has-text-align-left\" data-align=\"left\">760-845<\/td><td class=\"has-text-align-left\" data-align=\"left\">1400-1550<\/td><td class=\"has-text-align-left\" data-align=\"left\">10-30<\/td><td class=\"has-text-align-left\" data-align=\"left\">B ou W<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-345<\/td><td class=\"has-text-align-left\" data-align=\"left\">350-650<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h3 class=\"wp-block-heading\">Notas e refer\u00eancias<\/h3>\n\n\n\n<ol class=\"wp-block-list\">\n<li>(a) O, t\u00eampera em \u00f3leo; A, resfriamento ao ar; S, t\u00eampera em banho de sal; W, t\u00eampera em \u00e1gua; B, t\u00eampera em salmoura.<\/li>\n\n<li>(b) Quando o aquecimento a alta temperatura \u00e9 realizado em banho de sal, a faixa de temperaturas deve ser cerca de 14 \u00b0C (25 \u00b0F) inferior \u00e0 indicada aqui.<\/li>\n\n<li>(c) Revenimento duplo recomendado por n\u00e3o menos de 1 h na temperatura a cada vez.<\/li>\n\n<li>(d) Revenimento triplo recomendado por n\u00e3o menos de 1 h na temperatura a cada vez.<\/li>\n\n<li>(e) Os tempos se aplicam ao tratamento t\u00e9rmico em forno aberto. Para <a href=\"https:\/\/aobosteel.com\/pt\/packing-compounds-annealing-tool-steel\/\">t\u00eampera em caixa<\/a>, uma regra comum \u00e9 aquecer 1,2 min por mm (30 min por in.) de se\u00e7\u00e3o transversal da caixa.<\/li>\n\n<li>(f) Prefer\u00edvel para ferramentas grandes para minimizar a descarboneta\u00e7\u00e3o.<\/li>\n\n<li>(g) Temperatura de cementa\u00e7\u00e3o.<\/li>\n\n<li>(h) Ap\u00f3s a cementa\u00e7\u00e3o.<\/li>\n\n<li>(i) Cementado conforme dureza da camada.<\/li>\n\n<li>(j) O P21 \u00e9 um a\u00e7o endurec\u00edvel por precipita\u00e7\u00e3o que possui um tratamento t\u00e9rmico que envolve tratamento de solubiliza\u00e7\u00e3o e envelhecimento em vez de endurecimento e revenimento.<\/li>\n\n<li>(k) Recomendado para ferramentas grandes e ferramentas com se\u00e7\u00f5es complexas.<\/li>\n<\/ol>\n\n\n\n<h3 class=\"wp-block-heading\">Escopo do Fornecimento e Nota de Refer\u00eancia T\u00e9cnica<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">A Aobo Steel fornece a\u00e7o para ferramentas em <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-annealed-condition\/\">condi\u00e7\u00e3o recozida<\/a> e n\u00e3o fornece servi\u00e7os finais de tratamento t\u00e9rmico, como endurecimento, t\u00eampera, tratamento criog\u00eanico ou revenimento.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os par\u00e2metros de tratamento t\u00e9rmico, os dados de dureza e as recomenda\u00e7\u00f5es de processo nesta refer\u00eancia s\u00e3o fornecidos como suporte t\u00e9cnico geral aos nossos clientes. Os resultados reais do tratamento t\u00e9rmico podem variar dependendo da capacidade do forno, do tamanho da se\u00e7\u00e3o transversal, da geometria da ferramenta, da condi\u00e7\u00e3o do material, das pr\u00e1ticas de t\u00eampera e do controle do processo. Os procedimentos finais de tratamento t\u00e9rmico e a valida\u00e7\u00e3o devem ser realizados pela unidade de tratamento t\u00e9rmico do cliente, de acordo com a aplica\u00e7\u00e3o espec\u00edfica da ferramenta e os requisitos de produ\u00e7\u00e3o.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">P\u00e1ginas de refer\u00eancia relacionadas<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-properties-chart\/\">tabela de propriedades do a\u00e7o ferramenta<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-hot-hardness-chart\/\">gr\u00e1fico de dureza a quente<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-forging-temperature-guide\/\">Guia de temperatura de forjamento<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/pt\/astm-grain-size-chart-tool-steel\/\">Gr\u00e1fico de tamanho de gr\u00e3o ASTM<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/pt\/steel-heat-color-chart\/\">Tabela de cores por temperatura<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-hardness-conversion-calculator\/\">Calculadora de convers\u00e3o de dureza<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-material-finder\/\">Localizador de materiais de a\u00e7o ferramenta<\/a> \u00b7 <a href=\"https:\/\/aobosteel.com\/pt\/tool-steel-size-change-in-heat-treatment\/\">varia\u00e7\u00e3o dimensional do a\u00e7o para ferramentas no tratamento t\u00e9rmico<\/a><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Fonte de dados: Manual da ASM, A\u00e7os para Ferramentas Forjadas (revisado por Alan M. Bayer, Teledyne Vasco, e Lee R. Walton, Latrobe Steel Company). Tabelas 8 e 9. Dados compilados a partir de refer\u00eancias p\u00fablicas e normas da ind\u00fastria.<\/p>","protected":false},"excerpt":{"rendered":"<p>Normalizing, Annealing, Hardening &amp; Tempering of Tool Steels Complete reference for heat-treating temperatures of all major tool steel grades, with both \u00b0C and \u00b0F values. The quench and temper schedule is also published as a standalone table in the hardening and tempering temperature chart, and the overall process sequence is covered in the tool steel [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":17168,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"disabled","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-17163","page","type-page","status-publish","has-post-thumbnail","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Tool Steel Annealing &amp; Normalizing Temperature Chart - AoboSteel<\/title>\n<meta name=\"description\" content=\"Find recommended annealing and normalizing temperatures for AISI, DIN, and JIS tool steels, including D2, H13, A2, O1, P20, M2, W1, and more. Includes hardness after annealing and cooling rate reference tables based on ASM data.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/pt\/tool-steel-annealing-normalizing-temperature-chart\/\" \/>\n<meta property=\"og:locale\" content=\"pt_BR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Tool Steel Annealing &amp; Normalizing Temperature Chart\" \/>\n<meta property=\"og:description\" content=\"Find recommended annealing and normalizing temperatures for AISI, DIN, and JIS tool steels, including D2, H13, A2, O1, P20, M2, W1, and more. Includes hardness after annealing and cooling rate reference tables based on ASM data.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/pt\/tool-steel-annealing-normalizing-temperature-chart\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-21T12:57:22+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png\" \/>\n\t<meta property=\"og:image:width\" content=\"1254\" \/>\n\t<meta property=\"og:image:height\" content=\"1254\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/png\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Est. tempo de leitura\" \/>\n\t<meta name=\"twitter:data1\" content=\"12 minutos\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Tool Steel Annealing &amp; Normalizing Temperature Chart\",\"datePublished\":\"2026-07-31T01:28:48+00:00\",\"dateModified\":\"2026-10-21T12:57:22+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/\"},\"wordCount\":2330,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/07\\\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png\",\"inLanguage\":\"pt-BR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/\",\"name\":\"Tool Steel Annealing &amp; Normalizing Temperature Chart - AoboSteel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/07\\\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png\",\"datePublished\":\"2026-07-31T01:28:48+00:00\",\"dateModified\":\"2026-10-21T12:57:22+00:00\",\"description\":\"Find recommended annealing and normalizing temperatures for AISI, DIN, and JIS tool steels, including D2, H13, A2, O1, P20, M2, W1, and more. Includes hardness after annealing and cooling rate reference tables based on ASM data.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/#breadcrumb\"},\"inLanguage\":\"pt-BR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/07\\\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/07\\\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png\",\"width\":1254,\"height\":1254},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-annealing-normalizing-temperature-chart\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Tool Steel Annealing &amp; Normalizing Temperature Chart\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"pt-BR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"pt-BR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/pt\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"Tabela de temperaturas de recozimento e normaliza\u00e7\u00e3o de a\u00e7os para ferramentas - AoboSteel","description":"Encontre as temperaturas recomendadas de recozimento e normaliza\u00e7\u00e3o para a\u00e7os ferramenta AISI, DIN e JIS, incluindo D2, H13, A2, O1, P20, M2, W1 e outros. Inclui tabelas de refer\u00eancia de dureza ap\u00f3s recozimento e taxa de resfriamento com base em dados da ASM.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/pt\/tool-steel-annealing-normalizing-temperature-chart\/","og_locale":"pt_BR","og_type":"article","og_title":"Tool Steel Annealing &amp; Normalizing Temperature Chart","og_description":"Find recommended annealing and normalizing temperatures for AISI, DIN, and JIS tool steels, including D2, H13, A2, O1, P20, M2, W1, and more. Includes hardness after annealing and cooling rate reference tables based on ASM data.","og_url":"https:\/\/aobosteel.com\/pt\/tool-steel-annealing-normalizing-temperature-chart\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-21T12:57:22+00:00","og_image":[{"width":1254,"height":1254,"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png","type":"image\/png"}],"twitter_card":"summary_large_image","twitter_misc":{"Est. tempo de leitura":"12 minutos"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Tool Steel Annealing &amp; Normalizing Temperature Chart","datePublished":"2026-07-31T01:28:48+00:00","dateModified":"2026-10-21T12:57:22+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/"},"wordCount":2330,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png","inLanguage":"pt-BR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/","url":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/","name":"Tabela de temperaturas de recozimento e normaliza\u00e7\u00e3o de a\u00e7os para ferramentas - AoboSteel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png","datePublished":"2026-07-31T01:28:48+00:00","dateModified":"2026-10-21T12:57:22+00:00","description":"Encontre as temperaturas recomendadas de recozimento e normaliza\u00e7\u00e3o para a\u00e7os ferramenta AISI, DIN e JIS, incluindo D2, H13, A2, O1, P20, M2, W1 e outros. Inclui tabelas de refer\u00eancia de dureza ap\u00f3s recozimento e taxa de resfriamento com base em dados da ASM.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/#breadcrumb"},"inLanguage":"pt-BR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/"]}]},{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png","width":1254,"height":1254},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-annealing-normalizing-temperature-chart\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Tool Steel Annealing &amp; Normalizing Temperature Chart"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"AoboSteel","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"pt-BR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"AoboSteel","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"Evan","image":{"@type":"ImageObject","inLanguage":"pt-BR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png",1254,1254,false],"thumbnail":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels-150x150.png",150,150,true],"medium":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels-300x300.png",300,300,true],"medium_large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels-768x768.png",768,768,true],"large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels-1024x1024.png",1024,1024,true],"1536x1536":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png",1254,1254,false],"2048x2048":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png",1254,1254,false],"trp-custom-language-flag":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels-12x12.png",12,12,true]},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Normalizing, Annealing, Hardening &amp; Tempering of Tool Steels Complete reference for heat-treating temperatures of all major tool steel grades, with both \u00b0C and \u00b0F values. The quench and temper schedule is also published as a standalone table in the hardening and tempering temperature chart, and the overall process sequence is covered in the tool steel&hellip;","rttpg_featured_image_url":{"full":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png",1254,1254,false],"landscape":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png",1254,1254,false],"portraits":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png",1254,1254,false],"thumbnail":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels-150x150.png",150,150,true],"medium":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels-300x300.png",300,300,true],"large":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels-1024x1024.png",1024,1024,true],"1536x1536":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png",1254,1254,false],"2048x2048":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels.png",1254,1254,false],"trp-custom-language-flag":["https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/07\/Normalizing-Annealing-Hardening-Tempering-of-Tool-Steels-12x12.png",12,12,true]},"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/pt\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Normalizing, Annealing, Hardening &amp; Tempering of Tool Steels Complete reference for heat-treating temperatures of all major tool steel grades, with both \u00b0C and \u00b0F values. The quench and temper schedule is also published as a standalone table in the hardening and tempering temperature chart, and the overall process sequence is covered in the tool steel&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/17163","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/comments?post=17163"}],"version-history":[{"count":21,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/17163\/revisions"}],"predecessor-version":[{"id":23975,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/pages\/17163\/revisions\/23975"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media\/17168"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/pt\/wp-json\/wp\/v2\/media?parent=17163"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}