{"id":21317,"date":"2026-10-08T12:18:55","date_gmt":"2026-10-08T04:18:55","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=21317"},"modified":"2026-10-16T16:22:58","modified_gmt":"2026-10-16T08:22:58","slug":"tool-steel-band-sawing-speeds","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/tool-steel-band-sawing-speeds\/","title":{"rendered":"\ubc34\ub4dc \ud1b1 \uc808\ub2e8 \uacf5\uad6c\uac15, \uc808\ub2e8 \ubc0f \uc724\uacfd \uc18d\ub3c4"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\ubc34\ub4dc \ud1b1 \uc808\ub2e8 \uacf5\uad6c\uac15, \uc808\ub2e8 \ubc0f \uc724\uacfd \uc18d\ub3c4<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\ud1b1\uc9c8\uc740 \uacf5\uad6c\uac15 \ubd09\uc7ac\ub97c \uae38\uc774\uc5d0 \ub9de\uac8c \uc808\ub2e8\ud558\uace0 \ub2e4\uc774 \ube14\ub85d\uc744 \ub2e4\ub978 \uae30\uacc4 \uac00\uacf5 \uc804\uc5d0 \ud669\uc0ad\ud558\ub294 \ubc29\ubc95\uc785\ub2c8\ub2e4. \ubc34\ub4dc \ud1b1\uc740 \uc587\uace0 \uc5f0\uc18d\uc801\uc778 \ub0a0\ub85c \uc774\ub97c \uc218\ud589\ud558\uba70, \uacf5\uad6c\uac15\uc5d0 \ub300\ud574 \uacf5\ud45c\ub41c \uc18d\ub3c4\ub294 \uacf5\uad6c\uac15\uc744 \ud558\ub098\uc758 \uc7ac\ub8cc\ub85c \ubcf4\ub294 \uac83\uc774 \uc544\ub2c8\ub77c \ub4f1\uae09\ubcc4\ub85c \uc124\uc815\ub429\ub2c8\ub2e4. \uc544\ub798 \ud45c\ub294 \uc808\ub2e8 \ud1b1\uc9c8\uacfc \uc724\uacfd \ud1b1\uc9c8\uc5d0 \ub300\ud55c \ud574\ub2f9 \uc18d\ub3c4\uc640 \uadf8\uc5d0 \ub9de\ub294 \ub0a0 \uc7ac\ub8cc \ubc0f \ubc34\ub4dc \ud3ed\uc744 \uc81c\uc2dc\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ubc34\ub4dc \ud1b1\uc774 \uc808\ub2e8\ud560 \uc218 \uc788\ub294 \uac83<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ub3d9\ub825 \ubc34\ub4dc \ud1b1\uc740 \uc57d 180~250 HB\uc758 \uacbd\ub3c4 \ubc94\uc704\uc5d0\uc11c \uac00\uc7a5 \uc798 \uc791\ub3d9\ud569\ub2c8\ub2e4. \uc57d 400 HB\uae4c\uc9c0\uc758 \uac15, \uc77c\ubd80 \ucf8c\uc0ad\uac15\uc740 450 HB\uae4c\uc9c0\ub3c4 \ud1b1\uc9c8\ud560 \uc218 \uc788\uc9c0\ub9cc \uc808\uc0ad \uc18d\ub3c4\ub97c \ub0ae\ucd94\uc5b4\uc57c \ud569\ub2c8\ub2e4. \ubc34\ub4dc \ud1b1\uc9c8\uc740 \ud65c\ud1b1\uc9c8\uc774\ub098 \uc6d0\ud615 \ud1b1\uc9c8\ubcf4\ub2e4 \uc587\uc740 \ub0a0\uc744 \uc0ac\uc6a9\ud558\uba70 \uc808\uc0ad \ud3ed(kerf)\uc774 \uc57d 1.6 mm(1\/16 in.)\ub85c \ub2e4\ub978 \ub450 \ubc29\ubc95\uc758 7.9 mm \ubc0f 9.5 mm\uc5d0 \ube44\ud574 \uc791\uc73c\ubbc0\ub85c \ud544\uc694\ud55c \ub3d9\ub825\uc774 \uc801\uace0 \uce69\uc73c\ub85c \ubcc0\ud558\ub294 \uc7ac\ub8cc\ub3c4 \uc801\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc724\uacfd \uae30\uacc4\uc5d0\uc11c\ub294 \ub0a0\uc774 \uc9c1\uc120\uc774 \uc544\ub2cc \ud615\uc0c1\uc744 \ub530\ub77c\uac08 \uc218\ub3c4 \uc788\uc73c\ubbc0\ub85c, \ubc34\ub4dc \ud1b1\uc740 \ub2e4\uc774 \uc724\uacfd\uc744 \ubc00\ub9c1 \ub300\uc2e0 \uc5ec\ub7ec \uc139\uc158\uc73c\ub85c \ud669\uc0ad\ud558\ub294 \ub370 \uc790\uc8fc \uc0ac\uc6a9\ub429\ub2c8\ub2e4. \ub2e4\uc74c\uc5d0 \ub098\uc624\ub294 \uc18d\ub3c4\ub294 \uacf5\ud45c\ub41c \uc2e4\ubb34\uc5d0\uc11c \ub098\uc628 \uc2dc\uc791\uc810\uc774\uba70, \uac15\uc758 \ub4f1\uae09\uacfc \ub2e8\uba74 \ub450\uaed8\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9d1\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub4f1\uae09\ubcc4 \uc808\ub2e8 \ubc34\ub4dc \ud1b1\uc9c8 \uc18d\ub3c4<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc808\ub2e8 \ud1b1\uc9c8\uc5d0\uc11c \ubc34\ub4dc\ub294 \uc9c1\uc120 \uc808\ub2e8\ub9cc \ud558\uba70, \uc6d0\ubcf8 \ud45c\ub294 25 mm(1 in.) \ud3ed\uc758 \uace0\uc18d\ub3c4\uac15 \ubc34\ub4dc\uac00 \uc2a4\ucf00\uc77c \uc5c6\ub294 \uc9c1\uacbd 75~125 mm(3~5 in.)\uc758 \uc6d0\ud615\uc7ac\ub97c \uc808\ub2e8\ud558\ub294 \uac83\uc744 \uae30\uc900\uc73c\ub85c \ud569\ub2c8\ub2e4. \uc774\ub294 \ucd5c\ub300 450 mm(18 in.) \ub450\uaed8\uc758 \uace0\ud615 \ubd09\uc7ac\uc5d0 \uc801\uc6a9\ub429\ub2c8\ub2e4. \uc791\uc5c5\ubb3c\uc5d0 \uc2a4\ucf00\uc77c\uc774 \ub9ce\uc73c\uba74 \ubc34\ub4dc \uc18d\ub3c4\uc640 \uc808\uc0ad \uc18d\ub3c4\ub97c \ub0ae\ucd94\uc5b4\uc57c \ud558\uba70, \ud2b9\ud788 \uc587\uc740 \uc7ac\ub8cc\ub97c \uc808\ub2e8\ud560 \ub54c \ubc34\ub4dc \uc218\uba85\uc774 \ub2e8\ucd95\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4, HB<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubc34\ub4dc \uc18d\ub3c4, m\/min (sfm)<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc808\uc0ad \uc18d\ub3c4, mm<sup>2<\/sup> x 10<sup>3<\/sup>\/min (in.<sup>2<\/sup>\/min)<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubc34\ub4dc \uc218\uba85, mm<sup>2<\/sup> x 10<sup>6<\/sup> (in.<sup>2<\/sup> x 10<sup>3<\/sup>)<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">W1<\/td><td class=\"has-text-align-left\" data-align=\"left\">155-195<\/td><td class=\"has-text-align-left\" data-align=\"left\">67-55 (220-180)<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.9-3.2 (6-5)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.9 (3.0)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S2, S5<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">45-33 (150-110)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.6-1.9 (4-3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0 (1.5)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O1, O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">190-205<\/td><td class=\"has-text-align-left\" data-align=\"left\">65-55 (210-180)<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.9-2.6 (6-4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.6 (2.5)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-240<\/td><td class=\"has-text-align-left\" data-align=\"left\">60-52 (200-170)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.6-1.9 (4-3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.5 (2.3)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2, D3<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-240<\/td><td class=\"has-text-align-left\" data-align=\"left\">37-27 (120-90)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.9-1.3 (3-2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0 (1.5)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D7<\/td><td class=\"has-text-align-left\" data-align=\"left\">230-255<\/td><td class=\"has-text-align-left\" data-align=\"left\">27-18 (90-60)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.3-0.6 (2-1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.55 (0.85)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H12, H13, H21<\/td><td class=\"has-text-align-left\" data-align=\"left\">205-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">58-49 (190-160)<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.2-2.6 (5-4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.3 (2.0)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T1, T2<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-250<\/td><td class=\"has-text-align-left\" data-align=\"left\">40-30 (130-100)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.3-1.3 (3.5-2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.1 (1.7)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T6, T8<\/td><td class=\"has-text-align-left\" data-align=\"left\">220-295<\/td><td class=\"has-text-align-left\" data-align=\"left\">30-21 (100-70)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.6-0.6 (2.5-1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.7 (1.2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T15<\/td><td class=\"has-text-align-left\" data-align=\"left\">230-255<\/td><td class=\"has-text-align-left\" data-align=\"left\">23-15 (75-50)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.3-0.6 (2-1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.6 (1.0)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M1<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">45-37 (150-120)<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.2-1.9 (5-3)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.1 (1.7)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M2, M3<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-240<\/td><td class=\"has-text-align-left\" data-align=\"left\">33-24 (110-80)<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.6-1.3 (4-2)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.0 (1.5)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M4, M10, M15<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">27-18 (90-60)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.6-0.6 (2.5-1)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.7 (1.2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">190-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">55-49 (180-160)<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.9-2.6 (6-4)<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.6 (2.5)<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uacf5\uad6c\uac15\uc758 \uc808\ub2e8 \ubc34\ub4dc \ud1b1\uc9c8, ASM Handbook, Volume 16, Machining\uc758 Sawing Table 4\uc5d0\uc11c \uc7ac\ud604. \uc6d0\ubcf8 \ub370\uc774\ud130\ub294 25 mm(1 in.) \ud3ed\uc758 \uace0\uc18d\ub3c4\uac15 \ubc34\ub4dc, \uc77c\ubc18 \ud1b1\ub2c8 \ud615\ud0dc(\ub2e8, \uc57d 250 mm(10 in.)\ubcf4\ub2e4 \ub450\uaebc\uc6b4 \uae08\uc18d\uc5d0\ub294 \uac08\uace0\ub9ac \ud1b1\ub2c8 \ud615\ud0dc), raker set, \uc808\uc0ad \uc720\uccb4\ub97c \uc0ac\uc6a9\ud558\uc5ec \uc2a4\ucf00\uc77c \uc5c6\ub294 \ucd5c\ub300 460 mm(18 in.) \ub450\uaed8\uc758 \uace0\ud615 \ubd09\uc7ac\ub97c \uc808\ub2e8\ud558\ub294 \uac83\uc744 \uae30\uc900\uc73c\ub85c \ud569\ub2c8\ub2e4. D2, D3 \ubc0f D7\uc740 \uac74\uc2dd\uc73c\ub85c \uc808\ub2e8\ud569\ub2c8\ub2e4. \ubc34\ub4dc \uc218\uba85\uc740 3 m(10 ft) \ubc34\ub4dc\uc5d0 \ub300\ud574 \uc81c\uc2dc\ub418\uba70 \ub2e4\ub978 \ubc34\ub4dc \uae38\uc774\uc5d0 \ub300\ud574\uc11c\ub294 \ube44\ub840\ud569\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub4f1\uae09 \uac04\uc758 \ucc28\uc774\uac00 \uc774 \ud45c\uc758 \ud575\uc2ec\uc785\ub2c8\ub2e4. \uc800\ud569\uae08 \uc218\uacbd\ud654 \ubc0f \uc720\uacbd\ud654 \ub4f1\uae09\uc778 W1\uacfc O1\uc740 67~55 m\/min(220~180 sfm)\uc73c\ub85c \ud1b1\uc9c8\ub429\ub2c8\ub2e4. D2\uc640 D3\ub294 37~27 m\/min(120~90 sfm)\uc73c\ub85c, D7\uc740 27~18 m\/min(90~60 sfm)\uc73c\ub85c \ub5a8\uc5b4\uc9c0\uba70, \uc774 \uc138 \uac00\uc9c0\ub294 \uc720\uccb4 \uc5c6\uc774 \uac74\uc2dd\uc73c\ub85c \uc808\ub2e8\ub429\ub2c8\ub2e4. \uace0\uc18d\ub3c4 \ub4f1\uae09\uc740 \uc591 \ub05d \uc0ac\uc774\uc5d0 \uc704\uce58\ud558\uba70, T15\ub294 \uc804\uccb4 \uadf8\ub8f9 \uc911 \uac00\uc7a5 \ub290\ub9b0 23~15 m\/min(75~50 sfm)\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ubc34\ub4dc \uc218\uba85\ub3c4 \uac19\uc740 \uc21c\uc11c\ub97c \ub530\ub974\uba70 3 m(10 ft) \ubc34\ub4dc\uc5d0 \ub300\ud574 \uc81c\uc2dc\ub429\ub2c8\ub2e4. W1\uacfc O1\uc740 \uc57d 1.9 \ubc0f 1.6 \uc81c\uacf1\ubbf8\ud130\uc758 \uc808\ub2e8 \uba74\uc801\uc744, D2\uc640 D3\ub294 \uc57d 1.0, D7\uc740 0.55\ub9cc\uc744 \uc81c\uacf5\ud569\ub2c8\ub2e4. \ub9e4\uc77c D7\uc744 \uc808\ub2e8\ud558\ub294 \uc791\uc5c5\uc7a5\uc740 W1\uc744 \uc808\ub2e8\ud558\ub294 \uc791\uc5c5\uc7a5\ubcf4\ub2e4 \ubc34\ub4dc\ub97c \uba87 \ubc30 \ub354 \uc790\uc8fc \uad50\uccb4\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ub4f1\uae09 \ubc0f \ub450\uaed8\ubcc4 \uc724\uacfd \ubc34\ub4dc \ud1b1\uc9c8 \uc18d\ub3c4<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc724\uacfd \ud1b1\uc9c8\uc740 \ud615\uc0c1\uc744 \ub530\ub77c\uac00\uba70, \uc18d\ub3c4\ub294 \ub4f1\uae09\ubfd0\ub9cc \uc544\ub2c8\ub77c \uc808\ub2e8\ub418\ub294 \ub2e8\uba74\uc758 \ub450\uaed8\uc5d0 \uc758\ud574 \uc124\uc815\ub429\ub2c8\ub2e4. \ub3d9\uc77c\ud55c \ub4f1\uae09\uc774 \uc138 \uac00\uc9c0 \ub450\uaed8 \ubc94\uc704\uc5d0 \ub300\ud574 \ub098\uc5f4\ub418\uba70, \uba3c\uc800 \ud0c4\uc18c\uac15 \ubc34\ub4dc\ub85c, \uadf8\ub2e4\uc74c \uace0\uc18d\ub3c4\uac15 \ubc34\ub4dc\ub85c \uc81c\uc2dc\ub418\uc5b4 \uace0\uc18d\ub3c4 \ubc34\ub4dc\uc758 \uc774\uc810\uc744 \ubd84\uba85\ud788 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4. \uc587\uc740 \ubc94\uc704\uc5d0\uc11c W1\uc740 45 m\/min(150 sfm)\uc5d0\uc11c 82 m\/min(270 sfm)\uc73c\ub85c, O1\uc740 45\uc5d0\uc11c 80 m\/min\uc73c\ub85c \uc774\ub3d9\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud0c4\uc18c\uac15 \ubc34\ub4dc\ub294 \uacf5\uad6c\uac15\uc758 \uc724\uacfd \ud1b1\uc9c8\uc5d0 \uac00\uc7a5 \uc5f0\ud55c \ub4f1\uae09\uc5d0\uc11c\ub9cc, \uadf8\ub9ac\uace0 \uae30\uacc4\uc5d0 \uace0\uc18d\ub3c4 \ubc34\ub4dc\ub97c \uc704\ud55c \ub3d9\ub825\uacfc \uc720\uccb4 \uacf5\uae09\uc774 \ubd80\uc871\ud55c \uacbd\uc6b0\uc5d0\ub9cc \uad8c\uc7a5\ub429\ub2c8\ub2e4. \ub354 \ub2e8\ub2e8\ud55c \ub4f1\uae09\uc5d0\uc11c\ub294 \ud0c4\uc18c \ubc34\ub4dc \uac12\uc774 \ub5a8\uc5b4\uc9c0\uba70, D \ub4f1\uae09\uc740 \uc774\ubbf8 \uc587\uc740 \ubc94\uc704\uc5d0\uc11c 30 m\/min(100 sfm)\uae4c\uc9c0 \ub0ae\uc544\uc9d1\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>\ud0c4\uc18c\uac15 \ubc34\ub4dc<\/strong><\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4, HB<\/th><th class=\"has-text-align-left\" data-align=\"left\">6.4-13 mm (1\/4-1\/2 in.)<\/th><th class=\"has-text-align-left\" data-align=\"left\">25-75 mm (1-3 in.)<\/th><th class=\"has-text-align-left\" data-align=\"left\">150-300 mm (6-12 in.)<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">W1<\/td><td class=\"has-text-align-left\" data-align=\"left\">155-195<\/td><td class=\"has-text-align-left\" data-align=\"left\">45 (150)<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 (100)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S2, S5<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">24 (80)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O1, O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">185-205<\/td><td class=\"has-text-align-left\" data-align=\"left\">45 (150)<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 (100)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-240<\/td><td class=\"has-text-align-left\" data-align=\"left\">50 (170)<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 (100)<\/td><td class=\"has-text-align-left\" data-align=\"left\">20 (65)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2, D3<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-240<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 (100)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18 (60)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D7<\/td><td class=\"has-text-align-left\" data-align=\"left\">230-255<\/td><td class=\"has-text-align-left\" data-align=\"left\">24 (80)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H12, H13, H21<\/td><td class=\"has-text-align-left\" data-align=\"left\">205-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 (100)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18 (60)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T6, T8<\/td><td class=\"has-text-align-left\" data-align=\"left\">220-295<\/td><td class=\"has-text-align-left\" data-align=\"left\">27 (90)<\/td><td class=\"has-text-align-left\" data-align=\"left\">17 (55)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M4, M10, M15<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-240<\/td><td class=\"has-text-align-left\" data-align=\"left\">27 (90)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">190-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 (100)<\/td><td class=\"has-text-align-left\" data-align=\"left\">20 (65)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uc7ac\ub8cc \ub450\uaed8\ubcc4 \uacf5\uad6c\uac15\uc758 \uc724\uacfd \ubc34\ub4dc \ud1b1\uc9c8, ASM Handbook, Volume 16, Machining\uc758 Sawing Table 7\uc5d0\uc11c \uc7ac\ud604. \uc18d\ub3c4\ub294 m\/min\uc774\uba70 \uad04\ud638 \uc548\uc5d0 sfm\uc774 \uc788\uc2b5\ub2c8\ub2e4. \ud0c4\uc18c\uac15 \ubc34\ub4dc \uac12\uc740 \uc587\uc740 \ubc94\uc704\uc5d0 \ub300\ud574 14 pitch\uc758 \uc77c\ubc18 \ud1b1\ub2c8 \ud615\ud0dc\uc640 \ucd5c\uc18c \uc774\uc1a1\ub825\uc744, \uc911\uac04 \ubc94\uc704\uc5d0 \ub300\ud574 6~8 pitch\uc758 \uc77c\ubc18 \ud1b1\ub2c8 \ud615\ud0dc\uc640 \ud3c9\uade0 \uc774\uc1a1\ub825\uc744, \ub450\uaebc\uc6b4 \ubc94\uc704\uc5d0 \ub300\ud574 3 pitch\uc758 \uac08\uace0\ub9ac \ud1b1\ub2c8 \ud615\ud0dc\uc640 \ucd5c\ub300 \uc774\uc1a1\ub825\uc744 \uc0ac\uc6a9\ud569\ub2c8\ub2e4. \uace0\uc18d\ub3c4 \ubc34\ub4dc \uac12\uc740 \uc6a9\uc811 \uc5d0\uc9c0 \uace0\uc18d\ub3c4\uac15 \ubc34\ub4dc\uc5d0\ub3c4 \uc801\ud569\ud558\uba70, 10 pitch\uc758 \uc77c\ubc18 \ud1b1\ub2c8 \ud615\ud0dc\uc640 \ucd5c\uc18c \uc774\uc1a1\ub825, \uadf8\ub2e4\uc74c 6 pitch\uc758 \uc77c\ubc18 \ud1b1\ub2c8 \ud615\ud0dc\uc640 \ud3c9\uade0 \uc774\uc1a1\ub825, \uadf8\ub2e4\uc74c 3 pitch\uc758 \uac08\uace0\ub9ac \ud1b1\ub2c8 \ud615\ud0dc\uc640 \ucd5c\ub300 \uc774\uc1a1\ub825\uc744 \uc0ac\uc6a9\ud569\ub2c8\ub2e4. D2, D3 \ubc0f D7\uc740 \uac74\uc2dd\uc73c\ub85c \ud1b1\uc9c8\ub418\uba70, \uc6d0\ubcf8\uc5d0\uc11c \uac01\uc8fc\uac00 \uc788\ub294 \ub4f1\uae09\uc740 \uac01 \ubc94\uc704\uc5d0 \ub300\ud574 \ub354 \ubb34\uac70\uc6b4 \uc774\uc1a1\ub825\uc73c\ub85c \uc791\ub3d9\ud569\ub2c8\ub2e4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>\uace0\uc18d\ub3c4\uac15 \ubc34\ub4dc<\/strong><\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub4f1\uae09<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacbd\ub3c4, HB<\/th><th class=\"has-text-align-left\" data-align=\"left\">6.4-13 mm (1\/4-1\/2 in.)<\/th><th class=\"has-text-align-left\" data-align=\"left\">25-75 mm (1-3 in.)<\/th><th class=\"has-text-align-left\" data-align=\"left\">150-300 mm (6-12 in.)<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">W1<\/td><td class=\"has-text-align-left\" data-align=\"left\">155-195<\/td><td class=\"has-text-align-left\" data-align=\"left\">82 (270)<\/td><td class=\"has-text-align-left\" data-align=\"left\">55 (180)<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 (100)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">S2, S5<\/td><td class=\"has-text-align-left\" data-align=\"left\">175-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">58 (190)<\/td><td class=\"has-text-align-left\" data-align=\"left\">37 (120)<\/td><td class=\"has-text-align-left\" data-align=\"left\">18 (60)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">O1, O2<\/td><td class=\"has-text-align-left\" data-align=\"left\">185-205<\/td><td class=\"has-text-align-left\" data-align=\"left\">80 (260)<\/td><td class=\"has-text-align-left\" data-align=\"left\">55 (180)<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 (100)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">A2<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-240<\/td><td class=\"has-text-align-left\" data-align=\"left\">76 (250)<\/td><td class=\"has-text-align-left\" data-align=\"left\">53 (175)<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 (100)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D2, D3<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-240<\/td><td class=\"has-text-align-left\" data-align=\"left\">45 (150)<\/td><td class=\"has-text-align-left\" data-align=\"left\">30 (100)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">D7<\/td><td class=\"has-text-align-left\" data-align=\"left\">230-255<\/td><td class=\"has-text-align-left\" data-align=\"left\">33 (110)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21 (70)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">H12, H13, H21<\/td><td class=\"has-text-align-left\" data-align=\"left\">205-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">73 (240)<\/td><td class=\"has-text-align-left\" data-align=\"left\">49 (160)<\/td><td class=\"has-text-align-left\" data-align=\"left\">27 (90)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">T6, T8<\/td><td class=\"has-text-align-left\" data-align=\"left\">220-295<\/td><td class=\"has-text-align-left\" data-align=\"left\">38 (125)<\/td><td class=\"has-text-align-left\" data-align=\"left\">24 (80)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">M4, M10, M15<\/td><td class=\"has-text-align-left\" data-align=\"left\">215-240<\/td><td class=\"has-text-align-left\" data-align=\"left\">33 (110)<\/td><td class=\"has-text-align-left\" data-align=\"left\">21 (70)<\/td><td class=\"has-text-align-left\" data-align=\"left\">15 (50)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">L6<\/td><td class=\"has-text-align-left\" data-align=\"left\">190-230<\/td><td class=\"has-text-align-left\" data-align=\"left\">70 (230)<\/td><td class=\"has-text-align-left\" data-align=\"left\">49 (160)<\/td><td class=\"has-text-align-left\" data-align=\"left\">27 (90)<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">\ubc34\ub4dc \uc7ac\ub8cc \ubc0f \ub0a0 \uc120\ud0dd<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ubc34\ub4dc\ub294 \ud0c4\uc18c\uac15 \ub610\ub294 \ubc14\uc774\uba54\ud0c8\uc785\ub2c8\ub2e4. \ubc14\uc774\uba54\ud0c8(\ubcf5\ud569) \uc720\ud615\uc740 \uace0\uc7a5\ub825 \uac15 \ubc31\uc5d0 \uc6a9\uc811\ub41c \uace0\uc18d\ub3c4\uac15 \uc808\uc0ad \uc5d0\uc9c0\ub97c \uac00\uc9c0\uba70, \uc774\ub7ec\ud55c \uc6a9\uc811 \uc5d0\uc9c0 \ubc34\ub4dc\ub294 \uc0dd\uc0b0 \uae30\uacc4\uc5d0\uc11c \ud0c4\uc18c\uac15 \ubc34\ub4dc\uc640 \uae30\uc874\uc758 \uc77c\uccb4\ud615 \uace0\uc18d\ub3c4\uac15 \ubc34\ub4dc\ub97c \ubaa8\ub450 \ub300\uccb4\ud588\uc2b5\ub2c8\ub2e4. \uc6a9\uc811 \uc5d0\uc9c0 \ubc34\ub4dc\uc758 \uc808\uc0ad \uc5d0\uc9c0\ub294 \uc77c\ubc18\uc801\uc73c\ub85c M2, Matrix 2 \ub610\ub294 M42 \uace0\uc18d\ub3c4\uac15\uc774\uba70, \uc774 \uc138 \uac00\uc9c0\ub294 \uae30\uacc4\uac00 \uc544\ub2c8\ub77c \uc791\uc5c5\uc5d0 \ub530\ub77c \uc120\ud0dd\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\" rowspan=\"2\">\ubc34\ub4dc<\/th><th class=\"has-text-align-left\" data-align=\"left\" colspan=\"8\">\uc870\uc131, %<\/th><th class=\"has-text-align-left\" data-align=\"left\" rowspan=\"2\">\ub0b4\uc5f4\uc131, &deg;C (&deg;F)<\/th><th class=\"has-text-align-left\" data-align=\"left\" colspan=\"2\">\uacbd\ub3c4, HRC<\/th><\/tr><tr><th class=\"has-text-align-left\" data-align=\"left\">C<\/th><th class=\"has-text-align-left\" data-align=\"left\">Si<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mn<\/th><th class=\"has-text-align-left\" data-align=\"left\">Cr<\/th><th class=\"has-text-align-left\" data-align=\"left\">V<\/th><th class=\"has-text-align-left\" data-align=\"left\">W<\/th><th class=\"has-text-align-left\" data-align=\"left\">Mo<\/th><th class=\"has-text-align-left\" data-align=\"left\">Co<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud1b1\ub2c8<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubcf8\uccb4<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">M-2 \uace0\uc18d\ub3c4 \uc6a9\uc811 \uc5d0\uc9c0 \ubc34\ub4dc<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.79-0.86<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.35<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.95<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">. . .<\/td><td class=\"has-text-align-left\" data-align=\"left\">540 (1000)<\/td><td class=\"has-text-align-left\" data-align=\"left\">64-66<\/td><td class=\"has-text-align-left\" data-align=\"left\">40-47<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Matrix 2 \ubc34\ub4dc<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.70-0.78<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.30<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">590 (1100)<\/td><td class=\"has-text-align-left\" data-align=\"left\">65-67<\/td><td class=\"has-text-align-left\" data-align=\"left\">40-47<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ucf54\ubc1c\ud2b8 M-42 \ubc34\ub4dc<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.05-1.10<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.25<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.75<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.15<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.50<\/td><td class=\"has-text-align-left\" data-align=\"left\">8.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">700 (1300)<\/td><td class=\"has-text-align-left\" data-align=\"left\">67-69<\/td><td class=\"has-text-align-left\" data-align=\"left\">40-47<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ubc34\ub4dc \ud1b1\ub0a0 \uc870\uc131, ASM Handbook, Volume 16, Machining\uc758 Sawing Table 2\uc5d0\uc11c \uc7ac\ud604. \ub0b4\uc5f4\uc131\uc740 \uc808\uc0ad\ub0a0\uc774 \uacbd\ub3c4\ub97c \uc720\uc9c0\ud558\ub294 \uc628\ub3c4\uc774\ub2e4. \ubaa8\ub4e0 \uc6a9\uc811\ub0a0 \ubc34\ub4dc\uc758 \ubab8\uccb4\ub294 \ud1b1\ub2c8\uac00 \uacbd\ud654\ub41c \ud6c4 40~47 HRC\ub85c \uc791\ub3d9\ud558\ub294 \uace0\uc7a5\ub825 \ud569\uae08\uac15 \ubc31\uc774\ub2e4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud1b1\ub2c8 \ub05d \uacbd\ub3c4 64 HRC\uc758 M2\ub294 1.5 mm (0.060 in.) \ubbf8\ub9cc\uc758 \ub9e4\uc6b0 \uc587\uc740 \ubcbd \uac15\uad00\uacfc \ub9e4\uc6b0 \uc791\uc740 \ubd09\uc7ac\uc5d0 \uad8c\uc7a5\ub41c\ub2e4. \ud0c4\uc18c\uac15 \ubc0f \ud569\uae08\uac15\uc758 \uacbd\uc6b0 \ucd9c\ucc98\ub294 67 HRC\uc758 Matrix 2 \ub610\ub294 Matrix 2 \ub0a0\uc744 \uac00\uc9c4 \uac00\ubcc0 \ud53c\uce58 \ud1b1\ub0a0\uc744 \uad8c\uc7a5\ud55c\ub2e4. \uc5f4\ucc98\ub9ac\uac15, \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ubc0f \ucd08\ud569\uae08\uc758 \uacbd\uc6b0 69 HRC\uc758 M42 \ud1b1\ub2c8 \ub05d\uc774 \uad8c\uc7a5\ub418\uba70, M42 \ubc34\ub4dc\ub294 100 mm (4 in.) \uc774\uc0c1\uc758 \uc9c1\uacbd\uc744 \uc808\ub2e8\ud560 \ub54c \uc0ac\uc6a9\ud574\uc57c \ud55c\ub2e4. \ud574\ub2f9 \uc791\uc5c5\uc6a9 M42 \ud1b1\ub0a0\uc740 \ub354 \uc26c\uc6b4 \uce68\ud22c\ub97c \uc704\ud574 \ud45c\uc900 90\ub3c4 \ub798\uc774\ud06c \ub300\uc2e0 \ud3ec\uc9c0\ud2f0\ube0c \ub798\uc774\ud06c\ub97c \uac00\uc838\uc57c \ud55c\ub2e4. \ud569\uae08\uac15 \ubc31\uc5d0 \ube0c\ub808\uc774\uc9d5 \ub610\ub294 \uc6a9\uc811\ub41c \ud145\uc2a4\ud150 \uce74\ubc14\uc774\ub4dc \ub0a0\uc744 \uac00\uc9c4 \ubc34\ub4dc\ub294 \ucda9\uaca9 \uc800\ud56d\uc740 \ub0ae\uc9c0\ub9cc \uace0\uc628 \uacbd\ub3c4\uac00 \uac00\uc7a5 \ub192\uae30 \ub54c\ubb38\uc5d0 \ub2c8\ucf08 \ubc0f \ucf54\ubc1c\ud2b8 \uae30\ubc18 \ub0b4\uc5f4 \ud569\uae08\uacfc 150 mm (6 in.)\ubcf4\ub2e4 \ub450\uaebc\uc6b4 \ub2e8\uba74\uacfc \uac19\uc740 \uac00\uc7a5 \uc5b4\ub824\uc6b4 \uc791\uc5c5\uc6a9\uc73c\ub85c \uc720\uc9c0\ub41c\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc8fc\uc5b4\uc9c4 \ubc18\uacbd\uc5d0 \ub300\ud55c \ubc34\ub4dc \ud3ed<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc724\uacfd \uac00\uacf5\uae30\uc5d0\uc11c \ubc34\ub4dc\ub294 \uac78\ub9bc \uc5c6\uc774 \ubc18\uacbd\uc744 \ub530\ub77c\uc57c \ud558\uba70, \ubc34\ub4dc\uc758 \ud3ed\uc774 \uc808\ub2e8\ud560 \uc218 \uc788\ub294 \ucd5c\uc18c \ubc18\uacbd\uc744 \uacb0\uc815\ud55c\ub2e4. \ub354 \ub113\uc740 \ubc34\ub4dc\ub294 \ub354 \ub9ce\uc740 \ube54 \uac15\ub3c4\ub97c \uac00\uc9c0\uba70 \ub354 \uace7\uc740 \uc120\uc744 \uc720\uc9c0\ud558\ubbc0\ub85c, \uc5ec\uc804\ud788 \ubc18\uacbd\uc744 \uc808\ub2e8\ud560 \uc218 \uc788\ub294 \uac00\uc7a5 \ub113\uc740 \ubc34\ub4dc\uac00 \uc0ac\uc6a9\ud574\uc57c \ud560 \uac83\uc774\ub2e4. \ubaa8\ub4e0 \uc808\ub2e8\uc774 \uc9c1\uc120\uc778 \uc808\ub2e8 \uc791\uc5c5\uc5d0\uc11c\ub294 \ub354 \ub192\uc740 \ud558\uc911\uc744 \ubc1b\uae30 \ub54c\ubb38\uc5d0 \ud3ed 25~125 mm (1~5 in.)\uc758 \ubc34\ub4dc\uac00 \uc120\ud638\ub41c\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\" colspan=\"2\">\uc808\ub2e8\ud560 \ubc18\uacbd<\/th><th class=\"has-text-align-left\" data-align=\"left\" colspan=\"2\">\ubc34\ub4dc \ud3ed<\/th><\/tr><tr><th class=\"has-text-align-left\" data-align=\"left\">mm<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc548\uc5d0.<\/th><th class=\"has-text-align-left\" data-align=\"left\">mm<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc548\uc5d0.<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">&lt;1.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/16<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/16<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1.6<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/16<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">3\/32<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">3.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/8<\/td><td class=\"has-text-align-left\" data-align=\"left\">3.2<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">8<\/td><td class=\"has-text-align-left\" data-align=\"left\">5\/16<\/td><td class=\"has-text-align-left\" data-align=\"left\">4.8<\/td><td class=\"has-text-align-left\" data-align=\"left\">3\/16<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">5\/8<\/td><td class=\"has-text-align-left\" data-align=\"left\">6.4<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">36.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">1 7\/16<\/td><td class=\"has-text-align-left\" data-align=\"left\">9.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">3\/8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">65<\/td><td class=\"has-text-align-left\" data-align=\"left\">2 9\/16<\/td><td class=\"has-text-align-left\" data-align=\"left\">13<\/td><td class=\"has-text-align-left\" data-align=\"left\">1\/2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">95<\/td><td class=\"has-text-align-left\" data-align=\"left\">3 3\/4<\/td><td class=\"has-text-align-left\" data-align=\"left\">16<\/td><td class=\"has-text-align-left\" data-align=\"left\">5\/8<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">140<\/td><td class=\"has-text-align-left\" data-align=\"left\">5 1\/2<\/td><td class=\"has-text-align-left\" data-align=\"left\">19<\/td><td class=\"has-text-align-left\" data-align=\"left\">3\/4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">180<\/td><td class=\"has-text-align-left\" data-align=\"left\">7 1\/4<\/td><td class=\"has-text-align-left\" data-align=\"left\">25<\/td><td class=\"has-text-align-left\" data-align=\"left\">1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">300<\/td><td class=\"has-text-align-left\" data-align=\"left\">12<\/td><td class=\"has-text-align-left\" data-align=\"left\">32<\/td><td class=\"has-text-align-left\" data-align=\"left\">1 1\/4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">530<\/td><td class=\"has-text-align-left\" data-align=\"left\">21<\/td><td class=\"has-text-align-left\" data-align=\"left\">38<\/td><td class=\"has-text-align-left\" data-align=\"left\">1 1\/2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">710<\/td><td class=\"has-text-align-left\" data-align=\"left\">28<\/td><td class=\"has-text-align-left\" data-align=\"left\">50<\/td><td class=\"has-text-align-left\" data-align=\"left\">2<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ub2e4\uc591\ud55c \ubc18\uacbd\uc758 \uc724\uacfd \ud1b1\uc9c8\uc5d0 \uad8c\uc7a5\ub418\ub294 \ubc34\ub4dc \ud3ed, ASM Handbook, Volume 16, Machining\uc758 Sawing Table 3\uc5d0\uc11c \uc7ac\ud604.<\/em><\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uacf5\uad6c\uac15 \ubc34\ub4dc \ud1b1\uc9c8, \uc778\uc1c4 \uac00\ub2a5 PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">\uacf5\uad6c\uac15 \ub4f1\uae09\uc758 \uc808\ub2e8 \ubc0f \uc724\uacfd \ubc34\ub4dc \ud1b1\uc9c8 \uc18d\ub3c4, \ub0a0 \uc870\uc131 \ubc0f \ubc34\ub4dc \ud3ed \ud45c\ub97c \ub2f9\uc0ac \uc5f0\ub77d\ucc98\uc640 \ud568\uaed8 \ud558\ub098\uc758 PDF\ub85c \uc81c\uacf5.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Band-Sawing-Tool-Steel-Speeds.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<h2 class=\"wp-block-heading\">\ub4f1\uae09 \ubc0f \uc7ac\uace0<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud45c\uc5d0 \uc788\ub294 \ub450 \uace0\ud0c4\uc18c \uace0\ud06c\ub86c \ub4f1\uae09\uc740 \ub300\ubd80\ubd84\uc758 \uc791\uc5c5\uc7a5\uc5d0\uc11c \ubd09\uc7ac\ub85c \ud1b1\uc9c8\ud558\ub294 \ub4f1\uae09\uc774\uba70, \uc808\ub2e8 \ubc0f \uac00\uacf5 \uc18d\ub3c4\ub294 \ub2e4\uc74c\uc5d0 \uc81c\uc2dc\ub418\uc5b4 \uc788\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/d2-tool-steel-machining-guide\/\">D2 \uacf5\uad6c\uac15 \uac00\uacf5 \uac00\uc774\ub4dc<\/a>. \uacf5\uae30 \uacbd\ud654 \ub4f1\uae09\uacfc \uadf8 \ud1b1\uc9c8 \ubc0f \uac00\uacf5 \uac70\ub3d9\uc740 \ub2e4\uc74c\uc5d0 \uc788\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/a2-tool-steel-machining-fabrication-guide\/\">A2 \uacf5\uad6c\uac15 \uac00\uacf5 \ubc0f \uc81c\uc791 \uac00\uc774\ub4dc<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud06c\ub86c \uc5f4\uac04 \uac00\uacf5 \ub4f1\uae09\uc758 \uacbd\uc6b0 \ud1b1\uc9c8 \uc218\uce58\ub294 \uacbd\ud654 \ubc0f \uc0ac\uc6a9 \uacbd\ub3c4\uc640 \ud568\uaed8 \ub2e4\uc74c\uc5d0 \uc788\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/h13-tool-steel-machinability\/\">H13 \uacf5\uad6c\uac15 \uae30\uacc4\uac00\uacf5\uc131 \ud398\uc774\uc9c0<\/a>. \uc791\uc5c5\uc774 \ud1b1\uc5d0\uc11c \uc808\uc0ad \uacf5\uad6c\ub85c \uc774\ub3d9\ud558\ub294 \uacbd\uc6b0, \ub4f1\uae09\ubcc4 \uc120\uc0ad, \ubc00\ub9c1 \ubc0f \ub4dc\ub9b4\ub9c1 \uc18d\ub3c4\ub294 \ub2e4\uc74c\uc5d0 \uc218\uc9d1\ub418\uc5b4 \uc788\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-cutting-speeds-and-feeds\/\">\uacf5\uad6c\uac15 \uc808\uc0ad \uc18d\ub3c4 \ubc0f \uc774\uc1a1 \ud398\uc774\uc9c0<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud1b1\uc774 \ub0a8\uae30\ub294 \ub9c8\ubb34\ub9ac\ub294 \uc5f0\uc0ad \ud45c\uba74\uc774 \uc720\uc9c0\ud558\ub294 \uac83\ubcf4\ub2e4 \ud6e8\uc52c \uc6b0\uc218\ud558\uba70, \uac12\uc740 \uacf5\uc815\ubcc4\ub85c \ub2e4\uc74c\uc5d0 \ub098\uc5f4\ub418\uc5b4 \uc788\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/surface-roughness-chart\/\">\ud45c\uba74 \uac70\uce60\uae30 \ucc28\ud2b8<\/a>. \uc5f4\ucc98\ub9ac \ud6c4 \ub3d9\uc77c \ub4f1\uae09\uc740 \ud1b1\uc9c8 \ub300\uc2e0 \uc5f0\uc0ad\ub418\uba70, \ub4f1\uae09\ubcc4 \ud720 \uc120\ud0dd\uc740 \ub2e4\uc74c\uc5d0 \uc788\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-grindability-and-grinding-wheel-selection\/\">\uacf5\uad6c\uac15 \uc5f0\uc0ad\uc131 \ubc0f \uc5f0\uc0ad \ud720 \uc120\ud0dd \ud398\uc774\uc9c0<\/a>.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uacf5\uad6c\uac15 \ubc34\ub4dc \ud1b1\uc9c8, \uc778\uc1c4 \uac00\ub2a5 PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">\uacf5\uad6c\uac15 \ub4f1\uae09\uc758 \uc808\ub2e8 \ubc0f \uc724\uacfd \ubc34\ub4dc \ud1b1\uc9c8 \uc18d\ub3c4, \ub0a0 \uc870\uc131 \ubc0f \ubc34\ub4dc \ud3ed \ud45c\ub97c \ub2f9\uc0ac \uc5f0\ub77d\ucc98\uc640 \ud568\uaed8 \ud558\ub098\uc758 PDF\ub85c \uc81c\uacf5.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Band-Sawing-Tool-Steel-Speeds.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\">\uc774 \uac12\ub4e4\uc744 \uc0ac\uc6a9\ud558\uae30 \uc804\uc5d0<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \ud398\uc774\uc9c0\ub294 \uacf5\uac1c\ub41c \uad00\ud589\uc758 \ucc38\uc870 \uc694\uc57d\uc774\uba70 Aobo Steel \uc0ac\uc591\uc774 \uc544\ub2c8\ub2e4. \uc18d\ub3c4\ub294 \ucd9c\ucc98 \ud45c\uc5d0\uc11c \uc7ac\ud604\ub418\uc5c8\uc73c\uba70, \ub2e4\ub978 \ubc34\ub4dc, \ud1b1\ub2c8 \ud615\ud0dc, \uae30\uacc4 \ub610\ub294 \ubd09\uc7ac \uc0c1\ud0dc\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9c8 \uc218 \uc788\ub2e4. \ucd5c\uc885 \uc870\uac74\uc740 \ub0a9\ud488\ub41c \uc7ac\ub8cc\uc5d0 \ub9de\ucdb0 \uae30\uacc4\uc5d0\uc11c \uc124\uc815\ub41c\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Volume 16, Machining, ASM International, 1989.<\/p>","protected":false},"excerpt":{"rendered":"<p>Band Sawing Tool Steel, Cutoff and Contour Speeds Sawing is how a tool steel bar is cut to length and how a die block is roughed out before any other machining. A band saw does it with a thin, continuous blade, and the published speeds for tool steels are set grade by grade rather than [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-21317","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Band Sawing Tool Steel, Cutoff and Contour Speeds<\/title>\n<meta name=\"description\" content=\"Cutoff and contour band sawing speeds for tool steels by grade, with blade composition, tooth form and the band width for a given radius.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/tool-steel-band-sawing-speeds\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Band Sawing Tool Steel, Cutoff and Contour Speeds\" \/>\n<meta property=\"og:description\" content=\"Cutoff and contour band sawing speeds for tool steels by grade, with blade composition, tooth form and the band width for a given radius.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/tool-steel-band-sawing-speeds\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-16T08:22:58+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"9\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-band-sawing-speeds\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-band-sawing-speeds\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Band Sawing Tool Steel, Cutoff and Contour Speeds\",\"datePublished\":\"2026-10-08T04:18:55+00:00\",\"dateModified\":\"2026-10-16T08:22:58+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-band-sawing-speeds\\\/\"},\"wordCount\":1729,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-band-sawing-speeds\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-band-sawing-speeds\\\/\",\"name\":\"Band Sawing Tool Steel, Cutoff and Contour Speeds\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-08T04:18:55+00:00\",\"dateModified\":\"2026-10-16T08:22:58+00:00\",\"description\":\"Cutoff and contour band sawing speeds for tool steels by grade, with blade composition, tooth form and the band width for a given radius.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-band-sawing-speeds\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-band-sawing-speeds\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-band-sawing-speeds\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Band Sawing Tool Steel, Cutoff and Contour Speeds\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\ubc34\ub4dc \ud1b1 \uc808\ub2e8 \uacf5\uad6c\uac15, \uc808\ub2e8 \ubc0f \uc724\uacfd \uc18d\ub3c4","description":"\ub4f1\uae09\ubcc4 \uacf5\uad6c\uac15\uc758 \uc808\ub2e8 \ubc0f \uc724\uacfd \ubc34\ub4dc\uc18c \uc18d\ub3c4\uc640 \ud568\uaed8 \ub0a0 \uc7ac\uc9c8, \uce58\ud615, \uc8fc\uc5b4\uc9c4 \ubc18\uacbd\uc5d0 \ud544\uc694\ud55c \ubc34\ub4dc \ud3ed\uc744 \uc81c\uc2dc\ud569\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/tool-steel-band-sawing-speeds\/","og_locale":"ko_KR","og_type":"article","og_title":"Band Sawing Tool Steel, Cutoff and Contour Speeds","og_description":"Cutoff and contour band sawing speeds for tool steels by grade, with blade composition, tooth form and the band width for a given radius.","og_url":"https:\/\/aobosteel.com\/ko\/tool-steel-band-sawing-speeds\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-16T08:22:58+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"9\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-band-sawing-speeds\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-band-sawing-speeds\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Band Sawing Tool Steel, Cutoff and Contour Speeds","datePublished":"2026-10-08T04:18:55+00:00","dateModified":"2026-10-16T08:22:58+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-band-sawing-speeds\/"},"wordCount":1729,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-band-sawing-speeds\/","url":"https:\/\/aobosteel.com\/tool-steel-band-sawing-speeds\/","name":"\ubc34\ub4dc \ud1b1 \uc808\ub2e8 \uacf5\uad6c\uac15, \uc808\ub2e8 \ubc0f \uc724\uacfd \uc18d\ub3c4","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-08T04:18:55+00:00","dateModified":"2026-10-16T08:22:58+00:00","description":"\ub4f1\uae09\ubcc4 \uacf5\uad6c\uac15\uc758 \uc808\ub2e8 \ubc0f \uc724\uacfd \ubc34\ub4dc\uc18c \uc18d\ub3c4\uc640 \ud568\uaed8 \ub0a0 \uc7ac\uc9c8, \uce58\ud615, \uc8fc\uc5b4\uc9c4 \ubc18\uacbd\uc5d0 \ud544\uc694\ud55c \ubc34\ub4dc \ud3ed\uc744 \uc81c\uc2dc\ud569\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-band-sawing-speeds\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-band-sawing-speeds\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-band-sawing-speeds\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Band Sawing Tool Steel, Cutoff and Contour Speeds"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Band Sawing Tool Steel, Cutoff and Contour Speeds Sawing is how a tool steel bar is cut to length and how a die block is roughed out before any other machining. A band saw does it with a thin, continuous blade, and the published speeds for tool steels are set grade by grade rather than&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Band Sawing Tool Steel, Cutoff and Contour Speeds Sawing is how a tool steel bar is cut to length and how a die block is roughed out before any other machining. A band saw does it with a thin, continuous blade, and the published speeds for tool steels are set grade by grade rather than&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21317","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=21317"}],"version-history":[{"count":3,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21317\/revisions"}],"predecessor-version":[{"id":23220,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21317\/revisions\/23220"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=21317"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}