{"id":21295,"date":"2026-10-08T08:20:48","date_gmt":"2026-10-08T00:20:48","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=21295"},"modified":"2026-10-16T01:58:39","modified_gmt":"2026-10-15T17:58:39","slug":"permanent-mold-life-and-failure","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/permanent-mold-life-and-failure\/","title":{"rendered":"\uc601\uad6c \uae08\ud615 \uc218\uba85\uacfc \uc774\ub97c \ub2e8\ucd95\uc2dc\ud0a4\ub294 \uc694\uc778"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\uc601\uad6c \uae08\ud615 \uc218\uba85\uacfc \uc774\ub97c \ub2e8\ucd95\uc2dc\ud0a4\ub294 \uc694\uc778<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\uc601\uad6c \uae08\ud615\uc740 \ud234\ub9c1\uc774\uba70, \uc218\uba85\uc774 \uc815\ud558\ub294 \uc77c\uc815\uc5d0 \ub530\ub77c \uad50\uccb4 \ub610\ub294 \uc218\ub9ac\ub429\ub2c8\ub2e4. \uadf8 \uc218\uba85\uc740 100\ud68c \uc8fc\uc785\ubd80\ud130 250,000\ud68c\uae4c\uc9c0 \ub2e4\uc591\ud560 \uc218 \uc788\uc73c\uba70, \uacf5\uac1c\ub41c \uc9c0\uce68\uc5d0\uc11c\ub294 \uadf8 \ucc28\uc774\ub97c \uc18c\uc218\uc758 \uc6b4\uc804 \ubcc0\uc218\uc640 \uae08\ud615 \ubc0f \ucf54\uc5b4\uc758 \uc124\uacc4 \ubc29\uc2dd\uc73c\ub85c \uc124\uba85\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc601\uad6c \uae08\ud615\uc758 \uc218\uba85<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uae08\ud615 \uc218\uba85\uc740 \uc544\ub798\uc5d0 \uc81c\uc2dc\ub41c \ubcc0\uc218\uc5d0 \ub530\ub77c 100\ud68c \uc8fc\uc785\ubd80\ud130 250,000\ud68c \uc774\uc0c1\uae4c\uc9c0 \ub2e4\uc591\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc54c\ub8e8\ubbf8\ub284 \ud53c\uc2a4\ud1a4\uc6a9 \uae08\ud615\uc740 \uc218\ub9ac\uac00 \ud544\uc694\ud558\uae30 \uc804\uae4c\uc9c0 250,000\uac1c\uc758 \uc8fc\ubb3c\uc744 \uc0dd\uc0b0\ud560 \uac83\uc73c\ub85c \uc608\uc0c1\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ucd94\uac00\ub85c 250,000\uac1c\uc758 \uc8fc\ubb3c\uc744 \uc0dd\uc0b0\ud55c \ud6c4\uc5d0\ub294 \uc218\ub9ac\ub41c \uae08\ud615\uc5d0 \ub300\ub300\uc801\uc778 \uc815\ube44\uac00 \ud544\uc694\ud558\uba70, \ubc18\ubcf5\uc801\uc778 \uc218\ub9ac\uc640 \uc815\ube44\ub97c \uac70\uce58\uba74 \ud3d0\uae30\ub418\uae30 \uc804\uae4c\uc9c0 3.5\ubc31\ub9cc \uac1c\uc758 \uc8fc\ubb3c\uc744 \uc0dd\uc0b0\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud53c\uc2a4\ud1a4 \uae08\ud615\uc740 \uc124\uacc4\uac00 \ube44\uad50\uc801 \ub2e8\uc21c\ud558\uba70, \uc2e4\ub9b0\ub354 \ud5e4\ub4dc \uae08\ud615\ucc98\ub7fc \uc815\uad50\ud55c \ub0b4\ubd80 \ucf54\uc5b4\ub9c1\uacfc \uc678\ubd80 \uc778\uc11c\ud2b8\uac00 \ud544\uc694\ud55c \uae08\ud615\ubcf4\ub2e4 \ud6e8\uc52c \uc624\ub798 \uc0ac\uc6a9\ub429\ub2c8\ub2e4. \ub9c8\uadf8\ub124\uc298 \ud569\uae08\uc740 \uc720\uc0ac\ud55c \ud06c\uae30\uc640 \ud615\uc0c1\uc758 \uc54c\ub8e8\ubbf8\ub284 \ud569\uae08\ubcf4\ub2e4 \uae08\ud615\uc5d0 \ub354 \uc6b0\ud638\uc801\uc778\ub370, \uc6a9\uc735 \ub9c8\uadf8\ub124\uc298\uc774 \ucca0\uacc4 \uae08\ud615\uc744 \uce68\uc2dd\ud558\uc9c0 \uc54a\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \uadf8 \uc774\uc810\uc758 \ud06c\uae30\ub294 \uae08\ud615 \ucf54\ud305\uc774 \uc5bc\ub9c8\ub098 \uc798 \uc720\uc9c0\ub418\ub294\uc9c0\uc5d0 \ud06c\uac8c \uc88c\uc6b0\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uae08\ud615\uc740 \uc885\uc885 \uc8fc\ucca0\ub85c \ub9cc\ub4e4\uc5b4\uc9c0\ub294\ub370, \uc644\uc131 \ud615\uc0c1\uc5d0 \uac00\uae5d\uac8c \uae08\ud615\uc744 \uc8fc\uc870\ud558\uba74 \uac00\uacf5 \ube44\uc6a9\uc774 \uc808\uac10\ub418\uace0 \uc8fc\ucca0\uc774 \uac15\ubcf4\ub2e4 \uc6a9\uc735 \uc54c\ub8e8\ubbf8\ub284\uc758 \uce68\uc2dd\uc744 \ub354 \uc798 \uacac\ub514\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \uac15\uc740 \uc6a9\uc811\uc774 \uac00\ub2a5\ud558\uace0 \uc218\ub9ac\uac00 \ub354 \uc26c\uc6cc, \uac15 \uae08\ud615\uc740 \ub300\ub7c9 \uc0dd\uc0b0 \uc8fc\ubb3c\uc5d0 \uc790\uc8fc \uc0ac\uc6a9\ub429\ub2c8\ub2e4. \ud68c\uc8fc\ucca0 \uc8fc\uc870\uc5d0\uc11c\ub294 \uc720\uc0ac\ud55c \ud615\uc0c1\uc744 \uc54c\ub8e8\ubbf8\ub284 \ud569\uae08\uc73c\ub85c \uc8fc\uc870\ud558\ub294 \uacbd\uc6b0\uc5d0 \ube44\ud574 \uae08\ud615 \uc218\uba85\uc774 \uc9e7\uc744 \uac83\uc73c\ub85c \uc608\uc0c1\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uae08\ud615 \uc218\uba85\uc744 \ub2e8\ucd95\uc2dc\ud0a4\ub294 \ubcc0\uc218<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uacf5\uac1c\ub41c \uc8fc\uc694 \ubcc0\uc218 \ubaa9\ub85d\uc740 \uc8fc\uc785\ub418\ub294 \uae08\uc18d\ubd80\ud130 \uae08\ud615\uc758 \uc6b4\uc804 \ubc0f \ubcf4\uad00 \ubc29\uc2dd\uae4c\uc9c0 \uc774\uc5b4\uc9d1\ub2c8\ub2e4. \uadf8\uc911 \uc5ec\ub7ec \uac00\uc9c0\ub294 \uc7ac\ub8cc \uacb0\uc815\uc774 \uc544\ub2c8\ub77c \uc6b4\uc804 \uacb0\uc815\uc774\uba70, \uc7ac\ub8cc \uc120\ud0dd\ubcf4\ub2e4 \uc911\uc694\ub3c4\uac00 \ub192\uc2b5\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ubcc0\uc218<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uae08\ud615 \uc218\uba85\uc5d0 \ub300\ud55c \uc601\ud5a5<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc8fc\uc785 \uc628\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc8fc\uc870 \uae08\uc18d\uc744 \ub354 \ub728\uac81\uac8c \uc8fc\uc785\ud560\uc218\ub85d \uae08\ud615\uc774 \ub354 \ub728\uac81\uac8c \uc6b4\uc804\ub418\uc5b4 \uae08\ud615 \uae08\uc18d\uc774 \ube60\ub974\uac8c \uc57d\ud654\ub429\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc8fc\ubb3c \uc911\ub7c9<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc8fc\ubb3c \uc911\ub7c9\uc774 \uc99d\uac00\ud560\uc218\ub85d \uae08\ud615 \uc218\uba85\uc740 \uac10\uc18c\ud569\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc8fc\ubb3c \ud615\uc0c1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uae08\ud615 \ubcbd\uc740 \uc587\uc740 \ub2e8\uba74\uc758 \uc8fc\ubb3c\ubcf4\ub2e4 \ub450\uaebc\uc6b4 \ub2e8\uba74\uc758 \uc8fc\ubb3c\uc5d0\uc11c \ub354 \ub9ce\uc740 \uc5f4\uc744 \ubc1c\uc0b0\ud574\uc57c \ud569\ub2c8\ub2e4. \ub2e8\uba74 \ub450\uaed8\uc758 \ud070 \ubcc0\ud654\ub294 \uae08\ud615 \uc804\uccb4\uc5d0 \uc628\ub3c4 \ucc28\uc774\ub97c \ubc1c\uc0dd\uc2dc\ud0a4\uba70, \uadf8 \ucc28\uc774\uac00 \ucee4\uc9c8\uc218\ub85d \uae08\ud615 \uc218\uba85\uc740 \ub5a8\uc5b4\uc9d1\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub0c9\uac01 \ubc29\ubc95<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc218\ub0c9\uc740 \uacf5\ub7ad\ubcf4\ub2e4 \ub354 \ud6a8\uacfc\uc801\uc774\uc9c0\ub9cc \uae08\ud615 \uc218\uba85\uc744 \uc0c1\ub2f9\ud788 \uac10\uc18c\uc2dc\ud0b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uac00\uc5f4 \uc0ac\uc774\ud074<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uae08\ud615\uc744 \uade0\uc77c\ud55c \uc628\ub3c4\ub85c \uc720\uc9c0\ud558\ub294 \uc5f0\uc18d \uc6b4\uc804\uc774 \ucd5c\ub300 \uae08\ud615 \uc218\uba85\uc744 \uc81c\uacf5\ud569\ub2c8\ub2e4. \ub113\uc740 \ubc94\uc704\uc5d0 \uac78\uce5c \ubc18\ubcf5\uc801\uc778 \uac00\uc5f4\uacfc \ub0c9\uac01\uc740 \uc218\uba85\uc744 \ub2e8\ucd95\uc2dc\ud0b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uae08\ud615 \uc608\uc5f4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uac00\uc2a4 \ubd88\uaf43\uc774\ub098 \uc804\uae30 \ud788\ud130\ub85c \uc6b4\uc804 \uc628\ub3c4\uae4c\uc9c0 \uc608\uc5f4\ud558\uba74 \uae08\ud615 \uc218\uba85\uc774 \ud06c\uac8c \uc99d\uac00\ud569\ub2c8\ub2e4. \uc5f4\ucda9\uaca9\uc740 \uae08\ud615 \ud30c\uc190\uc758 \uc8fc\uc694 \uc6d0\uc778 \uc911 \ud558\ub098\uc785\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uae08\ud615 \ucf54\ud305<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucf54\ud305\uc740 \uae08\uc18d\uc774 \uae08\ud615 \ud45c\uba74\uc5d0 \ub2ff\uc9c0 \uc54a\ub3c4\ub85d \ud558\uc5ec \uce68\uc2dd\uacfc \uc6a9\ucc29\uc73c\ub85c\ubd80\ud130 \uae08\ud615\uc744 \ubcf4\ud638\ud558\uba70, \uae08\ud615 \uc218\uba85\uc744 \uc99d\uac00\uc2dc\ud0b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubab0\ub4dc \uc7ac\ub8cc<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacf5\uac1c\ub41c \uc120\ud0dd \ubaa9\ub85d\uc5d0\uc11c \uc120\ud0dd\ub41c \uc7ac\ub8cc\uac00 \uae08\ud615 \uc218\uba85\uc758 \uc0c1\ud55c\uc744 \uc815\ud569\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubcf4\uad00<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubd80\uc801\uc808\ud55c \ubcf4\uad00\uc740 \uae08\ud615 \ud45c\uba74\uc758 \ub179\uacfc \ud53c\ud305\uc744 \uc720\ubc1c\ud558\uc5ec \uae08\ud615 \uc218\uba85\uc744 \uac10\uc18c\uc2dc\ud0b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uccad\uc18c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f0\ub9c8 \ube14\ub77c\uc2a4\ud305, \uac00\uc131 \uc6a9\uc561 \uce68\uc9c0, \uc640\uc774\uc5b4 \ube0c\ub7ec\uc2f1\uc774 \ubaa8\ub450 \uc0ac\uc6a9\ub429\ub2c8\ub2e4. \uac00\uc131 \uc6a9\uc561\uc740 \uc791\uc5c5\uc790\uc5d0\uac8c \uc704\ud5d8\ud558\uba70, \ube14\ub77c\uc2a4\ud305\uacfc \ube0c\ub7ec\uc2f1\uc740 \uc8fc\uc758 \uae4a\uac8c \uad00\ub9ac\ud558\uc9c0 \uc54a\uc73c\uba74 \uacfc\ub3c4\ud55c \uae08\ud615 \ub9c8\ubaa8\ub97c \uc720\ubc1c\ud569\ub2c8\ub2e4. \uc720\ub9ac \ube44\ub4dc\ub294 \uac00\uc7a5 \uc548\uc804\ud55c \ube14\ub77c\uc2a4\ud2b8 \uc7ac\ub8cc\uc785\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uac8c\uc774\ud305<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubd88\ub7c9\ud55c \uac8c\uc774\ud305 \uc2dc\uc2a4\ud15c\uc740 \uac8c\uc774\ud2b8 \ubd80\uc704\uc5d0\uc11c \uacfc\ub3c4\ud55c \ub09c\ub958\uc640 \uc138\ucc99\uc744 \uc720\ubc1c\ud558\uc5ec \uae08\ud615 \uc218\uba85\uc744 \ud06c\uac8c \uac10\uc18c\uc2dc\ud0b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uae08\ud615 \uc6b4\uc804 \ubc29\ubc95<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc790\ub3d9 \ubc0f \uc218\ub3d9 \uc7a5\ube44\uc5d0 \ub3d9\uc77c\ud55c \uc7ac\ub8cc\uac00 \uc0ac\uc6a9\ub418\uc9c0\ub9cc, \uc218\ub3d9 \uc7a5\ube44\uc758 \ud234\ub9c1\uc740 \ud639\uc0ac\ub85c \uc778\ud574 \uc218\uba85\uc774 \ub354 \uc9e7\uc2b5\ub2c8\ub2e4. \uc790\ub3d9 \uc7a5\ube44\uc758 \ud234\ub9c1\uc740 \ucd5c\ub300 \ub450 \ubc30\uae4c\uc9c0 \ub354 \uc624\ub798 \uc9c0\uc18d\ub420 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc8fc\ubb3c\uc758 \ucd5c\uc885 \uc6a9\ub3c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc678\uad00\ubcf4\ub2e4 \uad6c\uc870\uc801 \uae30\ub2a5\uc774 \ub354 \uc911\uc694\ud55c \uacbd\uc6b0, \uae08\ud615\uc740 \ud3d0\uae30\ub418\uae30 \uc804\uae4c\uc9c0 \ub354 \ub9ce\uc740 \uc8fc\uc785 \ud69f\uc218 \ub3d9\uc548 \uc6b4\uc804\ub420 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uc601\uad6c \uae08\ud615\uc758 \uc218\uba85\uc5d0 \uc601\ud5a5\uc744 \ubbf8\uce58\ub294 \uc8fc\uc694 \ubcc0\uc218, ASM Handbook, Volume 15, Casting\uc758 Permanent Mold Casting \uae08\ud615 \uc218\uba85 \uc139\uc158\uc5d0\uc11c \ubc1c\ucdcc.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uadf8 \ubaa9\ub85d\uc5d0\uc11c \ub450 \ud56d\ubaa9\uc740 \ud2b9\ud788 \uc8fc\ubaa9\ud560 \uac00\uce58\uac00 \uc788\uc2b5\ub2c8\ub2e4. \uc218\ub0c9\uc740 \uacf5\ub7ad\ubcf4\ub2e4 \ub354 \ud6a8\uacfc\uc801\uc774\uc9c0\ub9cc \uae08\ud615 \uc218\uba85\uc744 \uc0c1\ub2f9\ud788 \uac10\uc18c\uc2dc\ud0a4\uba70, \uae08\ud615\uc744 \uc6b4\uc804 \uc628\ub3c4\uae4c\uc9c0 \uc608\uc5f4\ud558\uba74 \uc5f4\ucda9\uaca9\uc774 \uae08\ud615 \ud30c\uc190\uc758 \uc8fc\uc694 \uc6d0\uc778 \uc911 \ud558\ub098\uc774\uae30 \ub54c\ubb38\uc5d0 \uc218\uba85\uc774 \ud06c\uac8c \uc99d\uac00\ud569\ub2c8\ub2e4. \uade0\uc77c\ud55c \uc628\ub3c4\uc5d0\uc11c\uc758 \uc5f0\uc18d \uc6b4\uc804\uc774 \ucd5c\uc120\uc774\uba70, \ub113\uc740 \uc628\ub3c4 \ubc94\uc704\uc5d0 \uac78\uce5c \ubc18\ubcf5\uc801\uc778 \uc0ac\uc774\ud074\ub9c1\uc774 \ucd5c\uc545\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uae08\ud615 \uc124\uacc4\uac00 \uc218\uba85\uc744 \ub2e8\ucd95\uc2dc\ud0a4\ub294 \ubc29\uc2dd<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uae08\ud615 \uc124\uacc4\ub294 \uc6b4\uc804 \ubcc0\uc218 \uc678\uc5d0\ub3c4 \uc218\uba85\uc5d0 \ub69c\ub837\ud55c \uc601\ud5a5\uc744 \ubbf8\uce69\ub2c8\ub2e4. \uae08\ud615 \ubcbd \ub450\uaed8\uc758 \ubcc0\ud654\ub294 \uac00\uc5f4 \ubc0f \ub0c9\uac01 \uc911 \uacfc\ub3c4\ud55c \uc751\ub825\uc744 \uc720\ubc1c\ud558\uc5ec \uade0\uc5f4\uc5d0 \uc758\ud55c \uc870\uae30 \ud30c\uc190\uc744 \ucd08\ub798\ud558\uba70, \ucda9\ubd84\ud55c \ud544\ub81b \uc5c6\uc774 \ub450\uaed8\uac00 \uae09\uaca9\ud788 \ubcc0\ud558\ub294 \uacbd\uc6b0\ub3c4 \ub9c8\ucc2c\uac00\uc9c0\uc785\ub2c8\ub2e4. \uc791\uc740 \ud544\ub81b\uacfc \ub77c\ub514\uc6b0\uc2a4\ub294 \uac80\uc0ac, \uade0\uc5f4 \ubc0f \ucd5c\uc885 \ud30c\uc190\uc774 \uc885\uc885 \uadf8 \uc9c0\uc810\uc5d0\uc11c \uc2dc\uc791\ub418\uae30 \ub54c\ubb38\uc5d0 \uc218\uba85\uc744 \uac10\uc18c\uc2dc\ud0b5\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uad6c\ubc30\ub3c4 \uac19\uc740 \ub9e5\ub77d\uc758 \uc77c\ubd80\uc785\ub2c8\ub2e4. \uc8fc\ubb3c \uc218\ucd95 \ub54c\ubb38\uc5d0 \uc678\ubd80 \uae08\ud615 \ud45c\uba74\uc5d0\ub294 \ub0b4\ubd80 \ud45c\uba74\ubcf4\ub2e4 \ub354 \uc801\uc740 \uad6c\ubc30\uac00 \ud544\uc694\ud558\uba70, 5\ub3c4 \uad6c\ubc30\uac00 \ubc14\ub78c\uc9c1\ud569\ub2c8\ub2e4. \ub354 \ub0ae\uc740 \uad6c\ubc30 \uac01\ub3c4\ub294 \uae08\ud615 \uc218\ub9ac \uc0ac\uc774\uc5d0 \ub9cc\ub4e4 \uc218 \uc788\ub294 \uc8fc\ubb3c \uc218\ub97c \uac10\uc18c\uc2dc\ud0b5\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uae08\ud615 \ud45c\uba74<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uad6c\ubc30<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub0b4\ubd80 \uae08\ud615 \ud45c\uba74<\/td><td class=\"has-text-align-left\" data-align=\"left\">3\ub3c4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc678\ubd80 \uae08\ud615 \ud45c\uba74<\/td><td class=\"has-text-align-left\" data-align=\"left\">2\ub3c4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uad8c\uc7a5 \uc2e4\ubb34<\/td><td class=\"has-text-align-left\" data-align=\"left\">5\ub3c4<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uc601\uad6c \uae08\ud615\uc758 \uad6c\ubc30 \uac01\ub3c4, ASM Handbook, Volume 15, Casting\uc758 Permanent Mold Casting \uae08\ud615 \uc124\uacc4 \uc139\uc158\uc5d0\uc11c \ubc1c\ucdcc. \uc8fc\uc870 \uc218\ucd95 \ub54c\ubb38\uc5d0 \uc678\ubd80 \ud45c\uba74\uc5d0\ub294 \ub0b4\ubd80 \ud45c\uba74\ubcf4\ub2e4 \uc801\uc740 \uad6c\ubc30\uac00 \ud544\uc694\ud558\uba70, \uad6c\ubc30 \uac01\ub3c4\uac00 \ub0ae\uc744\uc218\ub85d \uae08\ud615 \uc218\ub9ac \uc0ac\uc774\uc5d0 \ub9cc\ub4e4 \uc218 \uc788\ub294 \uc8fc\ubb3c \uc218\uac00 \uc904\uc5b4\ub4e0\ub2e4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uae08\ud615 \uce90\ube44\ud2f0 \ub0b4\uc758 \ub3cc\ucd9c\ubd80\ub3c4 \uc218\uba85\uc744 \ub2e8\ucd95\ud55c\ub2e4. \uc774\ub4e4\uc740 \uadf9\ub3c4\ub85c \ub728\uac70\uc6cc\uc838 \uc8fc\ubb3c\uc744 \uc81c\uac70\ud560 \ub54c \uc555\ucd9c, \ubcc0\ud615 \ubc0f \uc190\uc0c1\uc758 \uc704\ud5d8\uc744 \ub192\uc778\ub2e4. \ub54c\ub85c\ub294 \uc778\uc11c\ud2b8\ub97c \uc0ac\uc6a9\ud558\uc5ec \ub9c8\ubaa8\ub418\uac70\ub098 \ud30c\uc190\ub41c \ub3cc\ucd9c\ubd80\ub97c \uad50\uccb4\ud558\uace0 \ub098\uba38\uc9c0 \uae08\ud615\uc758 \uc218\uba85\uc744 \uc5f0\uc7a5\ud560 \uc218 \uc788\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc5f4\uade0\uc5f4 \ubc0f \uae08\ud615 \uce68\uc2dd<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uae08\uc18d \ucda9\ub3cc\uacfc \uce90\ube44\ud14c\uc774\uc158\uc73c\ub85c \uc778\ud55c \uae08\ud615 \uce68\uc2dd\uc740 \ub458 \ub2e4 \ubd80\uc801\uc808\ud55c \uac8c\uc774\ud305 \uc124\uacc4\uc5d0\uc11c \ube44\ub86f\ub418\uba70, \uae08\ud615 \uae08\uc18d\uc758 \uae09\uc18d\ud55c \uc57d\ud654\uc640 \uc5f4\uade0\uc5f4\uc5d0 \uae30\uc5ec\ud55c\ub2e4. \uc774\ub7ec\ud55c \uc124\uacc4 \uc624\ub958\ub294 \uc7a5\uae30 \uc0dd\uc0b0 \uc911 \uae09\uaca9\ud55c \uce58\uc218 \ubcc0\ub3d9\uc73c\ub85c \ub098\ud0c0\ub09c\ub2e4. \ubd88\ucda9\ubd84\ud55c \uad6c\ubc30\ub098 \uc798\ubabb \uc124\uacc4\ub41c \uc774\uc81d\uc158 \uc2dc\uc2a4\ud15c\uc73c\ub85c \uc778\ud55c \uae30\uacc4\uc801 \ub9c8\ubaa8\ub3c4 \uac19\uc740 \uc601\ud5a5\uc744 \ubbf8\uce5c\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc5f4\uade0\uc5f4\uc740 \uae08\ud615 \uba74\uc774 \uacaa\ub294 \uc628\ub3c4 \uc0ac\uc774\ud074\uc5d0 \uc758\ud574 \uc0dd\uc131\ub418\ub294 \ud45c\uba74 \uade0\uc5f4 \ub124\ud2b8\uc6cc\ud06c\uc774\ub2e4. \uc774\ub294 \uad6c\ub9ac \ud569\uae08 \uc8fc\ubb3c\uc774 \ucd94\uac00\ud558\ub294 \ud30c\uc190 \ubaa8\ub4dc\uc778\ub370, \uc774\ub4e4\uc758 \ub354 \ub192\uc740 \uc8fc\uc785 \uc628\ub3c4\uac00 \uae08\ud615 \uce90\ube44\ud2f0\uc5d0 \ub354 \uc2ec\ud55c \uc0ac\uc774\ud074\ub9c1\uc744 \uac00\ud558\uae30 \ub54c\ubb38\uc774\ub2e4. \uc8fc\ubb3c\uc758 \ud45c\uba74\uc740 \uae08\ud615 \uce90\ube44\ud2f0\uc758 \ud45c\uba74\ubcf4\ub2e4 \ub098\uc744 \uc218 \uc5c6\uc73c\ubbc0\ub85c, \uae08\ud615\uc758 \uc5f4\uade0\uc5f4 \ubc0f \uae30\ud0c0 \uacb0\ud568\uc774 \uc8fc\ubb3c\uc5d0 \uc7ac\ud604\ub41c\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc0ac\uc6a9 \uc911 \uae08\ud615\uc744 \uc720\uc9c0\ud558\ub294 \uc694\uc18c<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uae08\ud615 \ucf54\ud305\uc740 \uc6a9\uc735 \uae08\uc18d\uacfc \uae08\ud615 \uc0ac\uc774\uc758 \uc7a5\ubcbd \uc5ed\ud560\uc744 \ud558\ub3c4\ub85d \uae08\ud615 \ubc0f \ucf54\uc5b4 \ud45c\uba74\uc5d0 \uc801\uc6a9\ub418\uba70, \uadf8\ub3d9\uc548 \uc751\uace0\ub41c \uae08\uc18d \ud53c\ub9c9\uc774 \ud615\uc131\ub41c\ub2e4. \uc774\ub294 \uc870\uae30 \uc751\uace0\ub97c \ubc29\uc9c0\ud558\uace0, \uc751\uace0 \uc18d\ub3c4\uc640 \ubc29\ud5a5\uc744 \uc81c\uc5b4\ud558\uba70, \uae08\ud615 \uc7ac\ub8cc\uc5d0 \ub300\ud55c \uc5f4\ucda9\uaca9\uc744 \ucd5c\uc18c\ud654\ud558\uace0, \uc6a9\uc735 \uae08\uc18d\uc774 \uae08\ud615\uc5d0 \uc6a9\ucc29\ub418\ub294 \uac83\uc744 \ubc29\uc9c0\ud558\uba70, \uce90\ube44\ud2f0\uc5d0 \uac07\ud78c \uacf5\uae30\ub97c \ubc30\ucd9c\ud558\uae30 \uc704\ud574 \uc0ac\uc6a9\ub41c\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc608\uc5f4\uc740 \ub2e4\ub978 \uc77c\uc0c1\uc801\uc778 \uc870\uce58\uc774\ub2e4. \uae08\ud615\uc740 \uc791\uc5c5 \uc2dc\uc791 \uc804\uc5d0 \ub300\ub7b5\uc801\uc778 \uc791\ub3d9 \uc628\ub3c4\ub85c \uc608\uc5f4\ub418\uba70, \uc774\ub294 \uc791\ub3d9 \uc628\ub3c4\uac00 \ud655\ub9bd\ub418\ub294 \ub3d9\uc548 \ub9cc\ub4e4\uc5b4\uc9c4 \ubd88\ub7c9 \uc8fc\ubb3c\uc758 \uc218\ub97c \uc904\uc778\ub2e4. \uc624\ube10\uc5d0\uc11c \uae08\ud615 \uba74\uc744 \uc608\uc5f4\ud558\ub294 \uac83\uc774 \uc5f4 \uad6c\ubc30\uac00 \ub354 \uc791\uae30 \ub54c\ubb38\uc5d0 \ucd5c\uc120\uc758 \ubc29\ubc95\uc774\uc9c0\ub9cc, \ub300\ud615 \uae08\ud615\uc5d0\ub294 \uc77c\ubc18\uc801\uc73c\ub85c \ube44\uc2e4\uc6a9\uc801\uc774\ub2e4.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uc601\uad6c \uae08\ud615 \uc218\uba85, \uc778\uc1c4 \uac00\ub2a5\ud55c PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">\uae08\ud615 \uc218\uba85 \ubc94\uc704, \uc774\ub97c \ub2e8\ucd95\uc2dc\ud0a4\ub294 \ubcc0\uc218 \ubc0f \uadf8\uc5d0 \ub530\ub978 \uad6c\ubc30 \uac01\ub3c4\ub97c \uc800\ud76c \uc5f0\ub77d\ucc98 \uc815\ubcf4\uc640 \ud568\uaed8 \ud558\ub098\uc758 PDF\ub85c \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Permanent-Mold-Life.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<h2 class=\"wp-block-heading\">\ub4f1\uae09 \ubc0f \uc7ac\uace0<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc601\uad6c \uae08\ud615 \ud234\ub9c1\uc5d0 \uc0ac\uc6a9\ub418\ub294 \uacf5\uad6c\uac15\uc740 \uc5f4\uac04 \uac00\uacf5 \ub4f1\uae09\uc785\ub2c8\ub2e4. \uac01\uac01\uc758 \uc138\ubd80 \uc0ac\ud56d\uc740 \ub2e4\uc74c\uc5d0 \uc788\uc2b5\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/h11-tool-steel\/\">H11 \ud234 \uc2a4\ud2f8 \ud398\uc774\uc9c0<\/a>, \uc544\uc5f0 \uae08\ud615\uacfc \uc54c\ub8e8\ubbf8\ub284 \ubc0f \ub9c8\uadf8\ub124\uc298 \ucf54\uc5b4\uc5d0 \uc0ac\uc6a9\ub418\ub294 \ubc94\uc6a9 \ud06c\ub86c \ub4f1\uae09\uc774\uba70, \ub2e4\uc74c\uc5d0\ub3c4 \uc788\uc2b5\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/h13-tool-steel\/\">H13 \ud234 \uc2a4\ud2f8 \ud398\uc774\uc9c0<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uae08\ud615 \uc218\uba85\uc758 \uc0c1\ud55c\uc744 \uc124\uc815\ud558\ub294 \uc7ac\ub8cc \uc120\ud0dd\uc740 \ub2e4\uc74c\uc5d0 \uc124\uba85\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/permanent-mold-and-core-materials\/\">\uc601\uad6c \uae08\ud615 \ubc0f \ucf54\uc5b4 \uc7ac\ub8cc \ud398\uc774\uc9c0<\/a>, \uc8fc\uc870 \ud569\uae08 \ubc0f \uc8fc\uc785 \ud69f\uc218\ubcc4\ub85c \uae08\ud615 \ubc0f \ucf54\uc5b4 \uc7ac\ub8cc\ub97c \ub098\uc5f4\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc5f4\uade0\uc5f4\uc740 \uac01 \uac80\uc0ac \uaddc\ubaa8\uc5d0\uc11c \uace0\uc720\ud55c \ud2b9\uc9d5\uc744 \uac00\uc9c4 \uc190\uc0c1 \ubaa8\ub4dc\uc774\uba70, \ub9c8\ubaa8 \ubc0f \uacfc\ubd80\ud558\uc640 \uad6c\ubcc4\ub418\ub294 \ubc29\uc2dd\uc740 \ub2e4\uc74c\uc5d0 \uc124\uba85\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/thermal-fatigue-resistant-tool-steels\/\">\ub0b4\uc5f4 \ud53c\ub85c \uacf5\uad6c\uac15 \ud398\uc774\uc9c0<\/a>. \uae08\ud615\uc774 \ud30c\uc190\ub418\uc5c8\uc744 \ub54c\uc758 \ubd84\uc11d \uacbd\ub85c\ub294, <a href=\"https:\/\/aobosteel.com\/ko\/tool-and-die-failure-analysis\/\">\uacf5\uad6c \ubc0f \ub2e4\uc774 \ud30c\uc190 \ubd84\uc11d \ud398\uc774\uc9c0<\/a> \uc5d0\uc11c \ud30c\uc190\uc774 \uc5b4\ub5bb\uac8c \ubd84\ub958\ub418\ub294\uc9c0 \ub2e4\ub8f9\ub2c8\ub2e4.<\/p>\n\n\n\n<div class=\"wp-block-group has-background is-layout-constrained wp-container-core-group-is-layout-3e4fb3d2 wp-block-group-is-layout-constrained\" style=\"border-radius:8px;background-color:#f4f8ff;margin-bottom:24px;padding-top:20px;padding-right:24px;padding-bottom:20px;padding-left:24px\">\n<p class=\"wp-block-paragraph\"><strong>\uc601\uad6c \uae08\ud615 \uc218\uba85, \uc778\uc1c4 \uac00\ub2a5\ud55c PDF<\/strong><\/p>\n\n<p class=\"wp-block-paragraph\">\uae08\ud615 \uc218\uba85 \ubc94\uc704, \uc774\ub97c \ub2e8\ucd95\uc2dc\ud0a4\ub294 \ubcc0\uc218 \ubc0f \uadf8\uc5d0 \ub530\ub978 \uad6c\ubc30 \uac01\ub3c4\ub97c \uc800\ud76c \uc5f0\ub77d\ucc98 \uc815\ubcf4\uc640 \ud568\uaed8 \ud558\ub098\uc758 PDF\ub85c \uc81c\uacf5\ud569\ub2c8\ub2e4.<\/p>\n\n<div class=\"wp-block-buttons is-layout-flex wp-block-buttons-is-layout-flex\">\n<div class=\"wp-block-button\"><a class=\"wp-block-button__link wp-element-button\" href=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Permanent-Mold-Life.pdf\">PDF \ub2e4\uc6b4\ub85c\ub4dc<\/a><\/div>\n\n<\/div>\n<\/div>\n\n\n\n<h3 class=\"wp-block-heading\">\uc774 \uac12\ub4e4\uc744 \uc0ac\uc6a9\ud558\uae30 \uc804\uc5d0<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \ud398\uc774\uc9c0\ub294 \uacf5\uac1c\ub41c \uc2e4\ubb34\uc5d0 \ub300\ud55c \ucc38\uc870 \uc694\uc57d\uc774\uba70 Aobo Steel\uc758 \uc0ac\uc591\uc774 \uc544\ub2d9\ub2c8\ub2e4. \uae08\ud615 \uc218\uba85 \uc218\uce58\ub294 \uc124\uba85\ub41c \ud569\uae08 \ubc0f \uacf5\uc815\uc5d0 \ub300\ud55c \uc77c\ubc18\uc801\uc778 \uacf5\uac1c \uac12\uc774\uba70, \ub2e4\ub978 \uc8fc\uc870 \ud569\uae08, \uae08\ud615 \uc124\uacc4 \ub610\ub294 \uc6b4\uc601 \uaddc\uc728\uc740 \uc774\ub97c \ubcc0\ud654\uc2dc\ud0b5\ub2c8\ub2e4. \uae08\ud615 \uad50\uccb4 \ubc0f \uc218\ub9ac\uc5d0 \ub300\ud55c \ucd5c\uc885 \uacb0\uc815\uc740 \uc8fc\ubb3c \ub3c4\uba74\uacfc \uc0dd\uc0b0 \uc77c\uc815\uc5d0 \ub530\ub77c \uc774\ub8e8\uc5b4\uc9d1\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Volume 15, Casting (9th Edition Metals Handbook), ASM International, 1988.<\/p>","protected":false},"excerpt":{"rendered":"<p>Permanent Mold Life and What Shortens It A permanent mold is tooling, and it is replaced or repaired on a schedule that its life sets. That life can be as few as 100 pours or as many as 250,000, and the published guidance puts the difference down to a short list of operating variables plus [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-21295","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.8 (Yoast SEO v28.8) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Permanent Mold Life: Variables and Failure Modes<\/title>\n<meta name=\"description\" content=\"What sets the life of a permanent mold, from 100 to 250,000 pours, with the operating variables and design points that shorten it.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/permanent-mold-life-and-failure\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Permanent Mold Life and What Shortens It\" \/>\n<meta property=\"og:description\" content=\"What sets the life of a permanent mold, from 100 to 250,000 pours, with the operating variables and design points that shorten it.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/permanent-mold-life-and-failure\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T17:58:39+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"7\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/permanent-mold-life-and-failure\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/permanent-mold-life-and-failure\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Permanent Mold Life and What Shortens It\",\"datePublished\":\"2026-10-08T00:20:48+00:00\",\"dateModified\":\"2026-10-15T17:58:39+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/permanent-mold-life-and-failure\\\/\"},\"wordCount\":1521,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/permanent-mold-life-and-failure\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/permanent-mold-life-and-failure\\\/\",\"name\":\"Permanent Mold Life: Variables and Failure Modes\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-08T00:20:48+00:00\",\"dateModified\":\"2026-10-15T17:58:39+00:00\",\"description\":\"What sets the life of a permanent mold, from 100 to 250,000 pours, with the operating variables and design points that shorten it.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/permanent-mold-life-and-failure\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/permanent-mold-life-and-failure\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/permanent-mold-life-and-failure\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Permanent Mold Life and What Shortens It\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\uc601\uad6c \uae08\ud615 \uc218\uba85: \ubcc0\uc218\uc640 \ud30c\uc190 \ubaa8\ub4dc","description":"100\ud68c\uc5d0\uc11c 250,000\ud68c \uc8fc\uc785\uae4c\uc9c0 \uc601\uad6c \uae08\ud615\uc758 \uc218\uba85\uc744 \uacb0\uc815\ud558\ub294 \uc694\uc778\uacfc \uc218\uba85\uc744 \ub2e8\ucd95\uc2dc\ud0a4\ub294 \uc6b4\uc804 \ubcc0\uc218 \ubc0f \uc124\uacc4 \uc0ac\ud56d\uc744 \ub2e4\ub8f9\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/permanent-mold-life-and-failure\/","og_locale":"ko_KR","og_type":"article","og_title":"Permanent Mold Life and What Shortens It","og_description":"What sets the life of a permanent mold, from 100 to 250,000 pours, with the operating variables and design points that shorten it.","og_url":"https:\/\/aobosteel.com\/ko\/permanent-mold-life-and-failure\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T17:58:39+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"7\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/permanent-mold-life-and-failure\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/permanent-mold-life-and-failure\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Permanent Mold Life and What Shortens It","datePublished":"2026-10-08T00:20:48+00:00","dateModified":"2026-10-15T17:58:39+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/permanent-mold-life-and-failure\/"},"wordCount":1521,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/permanent-mold-life-and-failure\/","url":"https:\/\/aobosteel.com\/permanent-mold-life-and-failure\/","name":"\uc601\uad6c \uae08\ud615 \uc218\uba85: \ubcc0\uc218\uc640 \ud30c\uc190 \ubaa8\ub4dc","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-08T00:20:48+00:00","dateModified":"2026-10-15T17:58:39+00:00","description":"100\ud68c\uc5d0\uc11c 250,000\ud68c \uc8fc\uc785\uae4c\uc9c0 \uc601\uad6c \uae08\ud615\uc758 \uc218\uba85\uc744 \uacb0\uc815\ud558\ub294 \uc694\uc778\uacfc \uc218\uba85\uc744 \ub2e8\ucd95\uc2dc\ud0a4\ub294 \uc6b4\uc804 \ubcc0\uc218 \ubc0f \uc124\uacc4 \uc0ac\ud56d\uc744 \ub2e4\ub8f9\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/permanent-mold-life-and-failure\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/permanent-mold-life-and-failure\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/permanent-mold-life-and-failure\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Permanent Mold Life and What Shortens It"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Permanent Mold Life and What Shortens It A permanent mold is tooling, and it is replaced or repaired on a schedule that its life sets. That life can be as few as 100 pours or as many as 250,000, and the published guidance puts the difference down to a short list of operating variables plus&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Permanent Mold Life and What Shortens It A permanent mold is tooling, and it is replaced or repaired on a schedule that its life sets. That life can be as few as 100 pours or as many as 250,000, and the published guidance puts the difference down to a short list of operating variables plus&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21295","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=21295"}],"version-history":[{"count":2,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21295\/revisions"}],"predecessor-version":[{"id":22715,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21295\/revisions\/22715"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=21295"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}