{"id":21191,"date":"2026-10-07T21:21:52","date_gmt":"2026-10-07T13:21:52","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=21191"},"modified":"2026-11-12T20:16:33","modified_gmt":"2026-11-12T12:16:33","slug":"stainless-steel-sensitization","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/stainless-steel-sensitization\/","title":{"rendered":"\uc2a4\ud14c\uc778\ub9ac\uc2a4 \uacf5\uad6c\uac15\uc758 \uc608\ubbfc\ud654 \ubc0f \uc785\uacc4 \ubd80\uc2dd"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\uc2a4\ud14c\uc778\ub9ac\uc2a4 \uacf5\uad6c\uac15\uc758 \uc608\ubbfc\ud654 \ubc0f \uc785\uacc4 \ubd80\uc2dd<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\uc785\uacc4\ub97c \ub530\ub77c \ud30c\uc190\ub41c \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uacf5\uad6c\uac15\uc740 \ub300\uac1c \ub3c4\uba74\uc0c1\uc758 \ubaa8\ub4e0 \uac80\uc0ac\ub97c \ud1b5\uacfc\ud588\uc2b5\ub2c8\ub2e4. \uac15\uc885\ub3c4 \ub9de\uace0 \uacbd\ub3c4\ub3c4 \ub9de\uace0 \ud45c\uba74\ub3c4 \uae68\ub057\ud588\uc2b5\ub2c8\ub2e4. \ubb38\uc81c\ub294 \uc5f4\ucc98\ub9ac \ub2e8\uacc4\uc5d0\uc11c \uac15\uc7ac\uac00 \ud2b9\uc815 \uc628\ub3c4 \ubc94\uc704\ub97c \ud1b5\uacfc\ud558\uac70\ub098 \uadf8\uacf3\uc5d0 \ub108\ubb34 \uc624\ub798 \uba38\ubb3c\ub7ec, \ubaa8\ub4e0 \uc785\uacc4 \uc606\uc758 \uae08\uc18d\uc5d0\uc11c \uac15\uc744 \uc2a4\ud14c\uc778\ub9ac\uc2a4\ub85c \ub9cc\ub4dc\ub294 \ud06c\ub86c\uc774 \ubd80\uc871\ud574\uc9c4 \uac83\uc785\ub2c8\ub2e4. \uc774 \ud398\uc774\uc9c0\ub294 \uadf8\ub7f0 \ud604\uc0c1\uc774 \uc5b8\uc81c \ubc1c\uc0dd\ud558\ub294\uc9c0, \ubd80\uc2dd \uc18d\ub3c4\uc5d0\uc11c \uc5b4\ub5a4 \ube44\uc6a9\uc774 \ub4dc\ub294\uc9c0, \uadf8\ub9ac\uace0 \uadf8 \uacb0\uacfc\uac00 \uc5b4\ub5bb\uac8c \uc2dc\ud5d8\ub418\uace0 \uc2b9\uc778\ub418\ub294\uc9c0\ub97c \ub2e4\ub8f9\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc774 \uc785\uacc4\ub97c \ub530\ub77c \ubd80\uc2dd\ub420 \uc218 \uc788\ub294 \uc774\uc720<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud06c\ub86c\uc740 \uac15\uc744 \uc2a4\ud14c\uc778\ub9ac\uc2a4\ub85c \ub9cc\ub4dc\ub294 \uc6d0\uc18c\uc785\ub2c8\ub2e4. \uc57d 1035 C (1900 F) \uc774\uc0c1\uc5d0\uc11c\ub294 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc758 \ud06c\ub86c \ud0c4\ud654\ubb3c\uc774 \uc644\uc804\ud788 \uc6a9\ud574\ub418\uc5b4, \ud06c\ub86c\uc774 \uace0\uc6a9\uccb4 \uc0c1\ud0dc\ub85c \uc874\uc7ac\ud558\uba70 \ud45c\uba74\uc744 \ubcf4\ud638\ud558\ub294 \ubd80\ub3d9\ud0dc \ud53c\ub9c9\uc744 \ud615\uc131\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uadf8 \uc628\ub3c4\uc5d0\uc11c \ucc9c\ucc9c\ud788 \ub0c9\uac01\ud558\uac70\ub098 425~815 C (800~1500 F)\ub85c \uc7ac\uac00\uc5f4\ud558\uba74 \ud0c4\ud654\ubb3c\uc774 \ub300\uc2e0 \uc785\uacc4\uc5d0 \uc11d\ucd9c\ub429\ub2c8\ub2e4. \uac01 \ud0c4\ud654\ubb3c\uc740 \uc8fc\ubcc0 \uae30\uc9c0\ubcf4\ub2e4 \ub354 \ub9ce\uc740 \ud06c\ub86c\uc744 \ud568\uc720\ud558\ubbc0\ub85c, \uc11d\ucd9c\uc740 \ubaa8\ub4e0 \uc785\uacc4 \uc591\ucabd\uc758 \uc881\uc740 \uc601\uc5ed\uc5d0\uc11c \ud06c\ub86c\uc744 \uace0\uac08\uc2dc\ud0b5\ub2c8\ub2e4. \uc774 \uc628\ub3c4\uc5d0\uc11c \ud06c\ub86c\uc740 \ub290\ub9ac\uac8c \ud655\uc0b0\ud558\ubbc0\ub85c \uace0\uac08 \uc601\uc5ed\uc740 \uadf8\ub300\ub85c \ub0a8\uc2b5\ub2c8\ub2e4. \uadf8\ub7ec\uba74 \uac15\uc740 \uc608\ubbfc\ud654\ub418\uc5b4, \uc785\uacc4\ub294 \uc6b0\uc120\uc801\uc73c\ub85c \ubd80\uc2dd\ub418\uace0 \uacb0\uc815\ub9bd \uc790\uccb4\ub294 \ubc1d\uac8c \uc720\uc9c0\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98\ub294 \uc774\uac83\uc774 \uc5bc\ub9c8\ub098 \uc911\uc694\ud55c\uc9c0\uc5d0 \uc218\uce58\ub97c \uc81c\uc2dc\ud569\ub2c8\ub2e4. \uc5fc\ud654\uc81c\uc774\ucca0\uc744 \ucca8\uac00\ud55c \ube44\ub4f1 50% \ud669\uc0b0\uc5d0\uc11c \ucca0-\ud06c\ub86c \ud569\uae08\uc740 \ud06c\ub86c \ud568\ub7c9\uc774 \uc99d\uac00\ud568\uc5d0 \ub530\ub77c \ubd80\uc2dd \uc18d\ub3c4\uac00 \uae09\uaca9\ud788 \uac10\uc18c\ud558\uba70, \uc774 \uc2dc\ud5d8\uc740 12~18% Cr \uc0ac\uc774\uc5d0\uc11c \uac00\uc7a5 \ubbfc\uac10\ud569\ub2c8\ub2e4. \uc774\ub294 \ubc14\ub85c \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uacf5\uad6c\uac15\uc774 \ucc28\uc9c0\ud558\ub294 \ud06c\ub86c \ubc94\uc704\uc774\ubbc0\ub85c, \uc785\uacc4\uc5d0\uc11c\uc758 \ud06c\ub86c \uc190\uc2e4\uc740 \uadf8 \uc2dc\ud5d8\uc774 \ub300\ud45c\ud558\ub294 \ud658\uacbd\uc5d0\uc11c \uc791\uc740 \uc601\ud5a5\uc774 \uc544\ub2d9\ub2c8\ub2e4. \ud06c\ub86c \uc218\uc900\uc774 \ub0ae\uc744\uc218\ub85d \ubd80\ub3d9\ud0dc \ud53c\ub9c9\uc774 \uc0b0\uc5d0 \ub354 \uc798 \uc6a9\ud574\ub418\ubbc0\ub85c, \ud53c\ub9c9\uc744 \ubcf5\uad6c\ud558\uae30 \uc704\ud574 \ub354 \ub9ce\uc740 \uae08\uc18d\uc774 \uc6a9\ud574\ub418\uc5b4\uc57c \ud558\uace0 \uce21\uc815\ub41c \ubd80\uc2dd \uc18d\ub3c4\uac00 \uc0c1\uc2b9\ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uac15\uc774 \uc0ac\uc774\ud074\uc5d0\uc11c \uc704\uce58\ud558\ub294 \uc9c0\uc810<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud0c4\ud654\ubb3c\uc774 \ud558\ub294 \uc77c<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uac15\uc5d0 \ub0a8\uae30\ub294 \uac83<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 1035 C (1900 F) \uc774\uc0c1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c \ud0c4\ud654\ubb3c\uc774 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uc5d0 \uc644\uc804\ud788 \uc6a9\ud574\ub428<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc785\uacc4\uc5d0 \ud06c\ub86c\uc774 \uc794\ub958\ud558\uc9c0 \uc54a\ub294 \uae68\ub057\ud55c \uc6a9\uccb4\ud654 \ucc98\ub9ac \uc870\uc9c1<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">1035 C \uc774\uc0c1\uc5d0\uc11c\uc758 \ub290\ub9b0 \ub0c9\uac01, \ub610\ub294 425~815 C (800~1500 F)\ub85c\uc758 \uc7ac\uac00\uc5f4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c \ud0c4\ud654\ubb3c\uc774 \uc785\uacc4\uc5d0 \uc11d\ucd9c\ub418\uba70, \uac01 \ud0c4\ud654\ubb3c\uc740 \uc8fc\ubcc0 \uae30\uc9c0\ubcf4\ub2e4 \ub354 \ub9ce\uc740 \ud06c\ub86c\uc744 \ud568\uc720\ud568<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubaa8\ub4e0 \uc785\uacc4 \uc606\uc758 \uae30\uc9c0\uac00 \ud06c\ub86c \uace0\uac08 \uc0c1\ud0dc\uac00 \ub418\uace0 \uac15\uc774 \uc608\ubbfc\ud654\ub428<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 675 C (1250 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c \ud0c4\ud654\ubb3c \uc11d\ucd9c \uc18d\ub3c4\uac00 \ucd5c\ub300\uac00 \ub418\ub294 \uc9c0\uc810<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc774 \ubc94\uc704\uc5d0\uc11c \uac00\uc7a5 \ub098\uc05c \uc9c0\uc810\uc774\uba70, \ud0c4\uc18c\uac15 \ubc0f \uc800\ud569\uae08\uac15\uc758 \uc77c\ubc18\uc801\uc778 \uc751\ub825 \uc81c\uac70 \uc628\ub3c4\uc784<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc57d 425 C (800 F) \uc774\ud558\ub85c \uc720\uc9c0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud0c4\ud654\ubb3c\uc774 \uc804\ud600 \uc11d\ucd9c\ub418\uc9c0 \uc54a\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc774 \uc218\uc900\uc744 \ube60\ub974\uac8c \ud1b5\uacfc\ud558\uc5ec \ub0c9\uac01\ud558\uba74 \uac15\uc740 \uc785\uacc4 \ubd80\uc2dd\uc5d0 \uba74\uc5ed\ub428<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc6a9\uc811\ubd80\uc758 \uc5f4\uc601\ud5a5\ubd80<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc6a9\uc811\ubd80 \uc790\uccb4\ub294 \ube60\ub974\uac8c \ub0c9\uac01\ub418\uc9c0\ub9cc, \uc601\uc5ed\uc758 \uc77c\ubd80\ub294 \uc11d\ucd9c \ubc94\uc704 \ub0b4\uc5d0 \ucda9\ubd84\ud788 \uc624\ub798 \uba38\ubb3c\ub7ec \ud0c4\ud654\ubb3c\uc744 \ud615\uc131\ud568<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc6a9\uc811 \uc5f4\ud654(weld decay)\ub85c, \uc608\ubbfc\ud654\uc758 \uc804\ud615\uc801\uc778 \ud604\uc7a5 \uc0ac\ub840\uc784<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98\uac00 \uc815\uc758\ud558\ub294 \uc608\ubbfc\ud654 \ubc94\uc704\uc785\ub2c8\ub2e4. \uac15\uc740 \uc6a9\uccb4\ud654 \uc628\ub3c4 \uc774\uc0c1\uc5d0\uc11c \uc548\uc804\ud558\uace0 \uc11d\ucd9c \ubc94\uc704 \uc774\ud558\uc5d0\uc11c\ub3c4 \uc548\uc804\ud558\uba70, \uc704\ud5d8\uc740 \uc804\uc801\uc73c\ub85c \ub0c9\uac01 \uacfc\uc815\uacfc \uc774\ud6c4 425~815 C\ub85c \ub2e4\uc2dc \uc9c4\uc785\ud558\ub294 \uc5f4\ucc98\ub9ac\uc5d0 \uc788\uc2b5\ub2c8\ub2e4. \ud574\ub2f9 \uae00\uc758 \uc785\uacc4 \ubd80\uc2dd \uc139\uc158\uc5d0\uc11c \ud3b8\uc9d1\ud568.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc57d 425 C (800 F)\ub97c \ube60\ub974\uac8c \ud1b5\uacfc\ud558\uc5ec \ub0c9\uac01\ud558\ub294 \uac83\uc774 \ub85c\uc5d0\uc11c\uc758 \ud574\ub2f5\uc785\ub2c8\ub2e4. \ud0c4\ud654\ubb3c\uc774 \ud615\uc131\ub420 \uc2dc\uac04\uc744 \uc804\ud600 \uc5bb\uc9c0 \ubabb\ud558\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \ud568\uc815\uc740 \uacbd\ud654 \ud6c4\uc758 \ub2e8\uacc4\uc785\ub2c8\ub2e4. \ud0c4\uc18c\uac15 \ubc0f \uc800\ud569\uae08\uac15\uc758 \uc751\ub825 \uc81c\uac70\ub294 \uc77c\ubc18\uc801\uc73c\ub85c \uc57d 675 C\uc5d0\uc11c \uc774\ub8e8\uc5b4\uc9c0\ub294\ub370, \uc774\ub294 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc5d0\uc11c \ud0c4\ud654\ubb3c \uc11d\ucd9c\uc774 \ucd5c\ub300\uac00 \ub418\ub294 \uc628\ub3c4\uc774\uae30\ub3c4 \ud558\ubbc0\ub85c, \uc751\ub825 \uc81c\uac70 \uc0ac\uc774\ud074\uc5d0\uc11c \ud0c4\uc18c\uac15 \ubd80\ud488\uacfc \ud568\uaed8 \uc7a5\uc785\ub41c \uc2a4\ud14c\uc778\ub9ac\uc2a4 \ubd80\ud488\uc740 \uc804\ud600 \uc758\ub3c4\ud558\uc9c0 \uc54a\uc740 \ucc98\ub9ac\uc5d0 \uc758\ud574 \uc608\ubbfc\ud654\ub420 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc6a9\uc811\ub3c4 \ub354 \uc791\uc740 \uaddc\ubaa8\ub85c \uac19\uc740 \uc77c\uc744 \uc77c\uc73c\ud0a4\ub294\ub370, \uc5f4\uc601\ud5a5\ubd80\ub294 \uc11d\ucd9c \ubc94\uc704\ub97c \ud1b5\uacfc\ud558\ub294 \ubc18\uba74 \uc6a9\uc735\ubd80 \uc790\uccb4\ub294 \uc774\ub97c \ud53c\ud560 \ub9cc\ud07c \ube60\ub974\uac8c \ub0c9\uac01\ub418\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud15c\ud37c\ub9c1\uc774 \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uacf5\uad6c\uac15\uc5d0 \ubbf8\uce58\ub294 \uc601\ud5a5<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uce7c\ub0a0, \uae08\ud615 \ubc0f \ub9c8\ubaa8 \ubd80\ud488\uc5d0 \uc0ac\uc6a9\ub418\ub294 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15\uc885\uc740 \ub2f4\uae08\uc9c8\ub85c \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uac00 \uc0dd\uc131\ub418\uc5b4 \uacbd\ud654\ub418\uba70, \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\ub294 \uc5f0\uc131\uc744 \ud68c\ubcf5\ud558\uae30 \uc704\ud574 \ud15c\ud37c\ub9c1\ud574\uc57c \ud569\ub2c8\ub2e4. \uc774 \ud15c\ud37c\ub9c1 \ub2e8\uacc4 \uc790\uccb4\uac00 \ud0c4\ud654\ubb3c\uc774 \ud615\uc131\ub418\ub294 \uc628\ub3c4 \ubc94\uc704\ub85c\uc758 \uc7ac\uac00\uc5f4\uc774\ubbc0\ub85c, \uacbd\ud654 \ubc0f \ud15c\ud37c\ub9c1\ub41c \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc758 \ub0b4\uc2dd\uc131\uc740 \uc131\ubd84 \ubd84\uc11d\ub9cc\uc774 \uc544\ub2c8\ub77c \ud15c\ud37c\ub9c1 \ubc29\uc2dd\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9d1\ub2c8\ub2e4. \ucd9c\ucc98\ub294 \ud398\ub77c\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc5d0 \ub300\ud55c \uad00\ub828 \uce21\uc815\uac12\uc744 \uae30\ub85d\ud558\ub294\ub370, 17% Cr \uac15\uc758 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8 \uc2dc\uc791 \uc628\ub3c4\ub294 176 C (349 F)\uc774\uace0 93 C (199 F)\uc5d0\uc11c \ubcc0\ud0dc\uac00 90% \uc644\ub8cc\ub418\uba70, 21% Cr \uac15\uc758 \uc2dc\uc791 \uc628\ub3c4\ub294 \uc601\ud558 160 C\uc774\uace0, \ub2f4\uae08\uc9c8\ub41c 25% Cr \ud569\uae08\uc5d0\uc11c\ub294 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uac00 \uc804\ud600 \uc5c6\uc2b5\ub2c8\ub2e4. \ud15c\ud37c\ub9c1\ub418\uc9c0 \uc54a\uc740 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\ub294 \uc778\uc131\uacfc \uc5f0\uc131\uc744 \ub5a8\uc5b4\ub728\ub9ac\uba70, \uc8fc\ubcc0 \uc870\uc9c1\ubcf4\ub2e4 \ub354 \ube60\ub974\uac8c \ubd80\uc2dd\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ub354 \ube60\ub974\uac8c \ubd80\uc2dd\ub418\ub294 \uc774\uc720\ub294 \uace0\uac1d\uacfc\uc758 \ub17c\uc758\uc5d0\uc11c \uc5b8\uae09\ud560 \uac00\uce58\uac00 \uc788\uc2b5\ub2c8\ub2e4. \ucca0-\ud06c\ub86c \ud569\uae08\uc774 \uace0\uc628\uc5d0\uc11c \ud398\ub77c\uc774\ud2b8\uc640 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\ub85c \ubd84\ub9ac\ub420 \ub54c, \ub450 \uc0c1\uc740 \uac19\uc740 \uc591\uc758 \ud06c\ub86c\uc744 \ubcf4\uc720\ud558\uc9c0 \uc54a\uc73c\uba70 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uac00 \ub458 \uc911 \ub354 \ub0ae\uc740 \ucabd\uc785\ub2c8\ub2e4. \uadf8 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uc5d0\uc11c \ud615\uc131\ub41c \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\ub294 \ub354 \ub0ae\uc740 \uc870\uc131\uc744 \ubb3c\ub824\ubc1b\uc73c\ubbc0\ub85c, \uc606\uc758 \ud398\ub77c\uc774\ud2b8\ubcf4\ub2e4 \ud06c\ub86c\uc774 \uc801\uc5b4 \ube44\ub4f1 \ud669\uc0b0 \uc2dc\ud5d8\uc5d0\uc11c \uba3c\uc800 \uc6a9\ud574\ub429\ub2c8\ub2e4. \ucd9c\ucc98\ub294 type 430\uc758 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uc5d0\uc11c \uc815\ud655\ud788 \uadf8\ub7f0 \uac70\ub3d9\uc744 \ubcf4\uace0\ud558\uba70, \ub354 \ub192\uc740 \ud06c\ub86c \uc218\uc900\uc5d0\uc11c\ub294 \uac19\uc740 \ucc28\uc774\uc5d0 \uc2dc\ud5d8\uc774 \ubbfc\uac10\ud558\uc9c0 \uc54a\ub2e4\uace0 \uc5b8\uae09\ud558\ub294\ub370, \uc774\uac83\uc774 type 446\uc5d0\uc11c \ud615\uc131\ub41c \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uc5d0\uc11c \uc6b0\uc120\uc801 \uce68\uc2dd\uc774 \ub098\ud0c0\ub098\uc9c0 \uc54a\uc740 \uc774\uc720\uc785\ub2c8\ub2e4. \uc27d\uac8c \ub9d0\ud574, \ud06c\ub86c\uc774 \uac00\uc7a5 \ub0ae\uc740 \uc0c1\uc774 \uac00\uc7a5 \uba3c\uc800 \ubd80\uc2dd\ub418\ub294 \uc0c1\uc774\uba70, \uc778\uc99d\uc11c\uc5d0 \uc801\ud78c \uac15\uc885\uba85\uc774 \ubb34\uc5c7\uc774\ub4e0 \ub9c8\ucc2c\uac00\uc9c0\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud06c\ub86c\uc744 \ube7c\uc557\ub294 \uc774\ucc28 \uc0c1<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud0c4\ud654\ubb3c\uc740 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc744 \uc628\ub3c4\uc5d0 \uc720\uc9c0\ud560 \ub54c \ud615\uc131\ub418\ub294 \uc0c1 \uc911 \uac00\uc7a5 \uc798 \uc54c\ub824\uc9c4 \uac83\uc77c \ubfd0\uc785\ub2c8\ub2e4. \ucd9c\ucc98\ub294 \uac01 \uc0c1\uc774 \ub098\ud0c0\ub098\ub294 \ubc94\uc704\uc640 \ud568\uaed8 \uc804\uccb4 \ubaa9\ub85d\uc744 \uc81c\uc2dc\ud558\uba70, \uc774\ub4e4\uc740 \uc5f4\ucc98\ub9ac \uc77c\uc815\uc5d0 \uc911\uc694\ud558\uac8c \uc791\uc6a9\ud558\ub294 \ubc29\uc2dd\uc73c\ub85c \uacb9\uce69\ub2c8\ub2e4. \uc2dc\uadf8\ub9c8 \uc0c1\uacfc \uce74\uc774 \uc0c1\uc740 \uac01\uac01 \ub300\ub7b5 550~1050 C (1020~1920 F)\uc640 600~900 C (1110~1650 F)\uc5d0\uc11c \ud615\uc131\ub418\uba70, \ub458 \ub2e4 \ub0b4\uc2dd\uc131\uc744 \uac10\uc18c\uc2dc\ud0a4\uace0 \uc5f0\uc131\uacfc \uc778\uc131\uc744 \ub5a8\uc5b4\ub728\ub9bd\ub2c8\ub2e4. \uc54c\ud30c \ud504\ub77c\uc784\uc740 \ud6e8\uc52c \ub0ae\uc740 \uc628\ub3c4\uc778 350~550 C (660~1020 F)\uc5d0\uc11c \ub098\ud0c0\ub098\ub294 \ud06c\ub86c\uc774 \ud48d\ubd80\ud55c \uc0c1\uc774\uba70, \ub0b4\uc2dd\uc131\uc5d0\ub294 \uac70\uc758 \uc601\ud5a5\uc774 \uc5c6\uc9c0\ub9cc \uadf8 \ud615\uc131\uc774 475 C \ucde8\ud654\ub85c \uc54c\ub824\uc9c4 \uc778\uc131 \uc190\uc2e4\uc758 \uc6d0\uc778\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc0c1<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc0c1\uc9d5<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc720\ud615<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uacf5\uc2dd<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubc94\uc704, C<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubc94\uc704, F<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c \ud0c4\ud654\ubb3c<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">M7C3<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Cr,Fe,Mo)7C3<\/td><td class=\"has-text-align-left\" data-align=\"left\">950~1050<\/td><td class=\"has-text-align-left\" data-align=\"left\">1740~1920<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c \ud0c4\ud654\ubb3c<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">M23C6<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Cr,Fe,Mo)23C6<\/td><td class=\"has-text-align-left\" data-align=\"left\">600 ~ 950<\/td><td class=\"has-text-align-left\" data-align=\"left\">1110 ~ 1740<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c \ud0c4\ud654\ubb3c<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">M6C<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Cr,Fe,MoNb)6C<\/td><td class=\"has-text-align-left\" data-align=\"left\">700 ~ 950<\/td><td class=\"has-text-align-left\" data-align=\"left\">1290 ~ 1740<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud06c\ub86c \uc9c8\ud654\ubb3c<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">M2N<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Cr,Fe)2N<\/td><td class=\"has-text-align-left\" data-align=\"left\">650 ~ 950<\/td><td class=\"has-text-align-left\" data-align=\"left\">1200 ~ 1740<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Fe-Mo \uc9c8\ud654\ubb3c<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">M5N<\/td><td class=\"has-text-align-left\" data-align=\"left\">Fe7Mo13N4<\/td><td class=\"has-text-align-left\" data-align=\"left\">550 ~ 600<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020 ~ 1110<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Nb-Cr \uc9c8\ud654\ubb3c<\/td><td class=\"has-text-align-left\" data-align=\"left\">Z<\/td><td class=\"has-text-align-left\" data-align=\"left\">MN<\/td><td class=\"has-text-align-left\" data-align=\"left\">(NbCr)N<\/td><td class=\"has-text-align-left\" data-align=\"left\">700 ~ 1000<\/td><td class=\"has-text-align-left\" data-align=\"left\">1290 ~ 1830<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub2c8\uc624\ube00 \ud0c4\uc9c8\ud654\ubb3c<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">MC<\/td><td class=\"has-text-align-left\" data-align=\"left\">Nb(CN)<\/td><td class=\"has-text-align-left\" data-align=\"left\">700 ~ \uc735\uc810<\/td><td class=\"has-text-align-left\" data-align=\"left\">1290 ~ \uc735\uc810<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc2dc\uadf8\ub9c8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u03c3<\/td><td class=\"has-text-align-left\" data-align=\"left\">AB<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Fe,Cr,Mo,Ni)<\/td><td class=\"has-text-align-left\" data-align=\"left\">550 ~ 1050<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020 ~ 1920<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uce74\uc774<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u03c7<\/td><td class=\"has-text-align-left\" data-align=\"left\">A48B10<\/td><td class=\"has-text-align-left\" data-align=\"left\">Fe36Cr12Mo10 over (FeNi)36Cr18(TiMo)4<\/td><td class=\"has-text-align-left\" data-align=\"left\">600 ~ 900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1110 ~ 1650<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc54c\ud30c \ud504\ub77c\uc784<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u03b1\u2032<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">Cr 61 ~ 83%\uc758 CrFe<\/td><td class=\"has-text-align-left\" data-align=\"left\">350 ~ 550<\/td><td class=\"has-text-align-left\" data-align=\"left\">660 ~ 1020<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub77c\ubca0\uc2a4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u03b7<\/td><td class=\"has-text-align-left\" data-align=\"left\">A2B<\/td><td class=\"has-text-align-left\" data-align=\"left\">(FeCr)2(Mo,Nb,Ti,Si)<\/td><td class=\"has-text-align-left\" data-align=\"left\">550 ~ 900<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020 ~ 1650<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">R<\/td><td class=\"has-text-align-left\" data-align=\"left\">R<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">(Fe,Mo,Cr,Ni)<\/td><td class=\"has-text-align-left\" data-align=\"left\">550 ~ 650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020 ~ 1200<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Tau<\/td><td class=\"has-text-align-left\" data-align=\"left\">\u03c4<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><td class=\"has-text-align-left\" data-align=\"left\">550 ~ 650<\/td><td class=\"has-text-align-left\" data-align=\"left\">1020 ~ 1200<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc758 2\ucc28 \uc0c1\uacfc \uac01 \uc0c1\uc774 \ud615\uc131\ub418\ub294 \uc628\ub3c4 \ubc94\uc704. \ucd9c\ucc98\uc758 \uc720\ud615 \ucf54\ub4dc\ub294 A\ub294 \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uacc4, D\ub294 \ub4c0\ud50c\ub809\uc2a4\uacc4, F\ub294 \ud398\ub77c\uc774\ud2b8\uacc4\ub97c \ub098\ud0c0\ub0b8\ub2e4. \ucd9c\ucc98: \ud574\ub2f9 \ub17c\ubb38\uc758 Table 8.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud574\ub2f9 \ud45c\uc758 \ub450 \ud56d\ubaa9\uc740 \uacf5\uad6c\uac15 \uc791\uc5c5\uc5d0\uc11c \uc8fc\ubaa9\ud560 \ub9cc\ud558\ub2e4. M7C3\uc640 M23C6 \ud06c\ub86c \ud0c4\ud654\ubb3c\uc740 \uadf8 \uc0ac\uc774\uc758 \ud15c\ud37c\ub9c1 \ubc94\uc704\ub97c \uc591\ubd84\ud558\uba70, M23C6\ub294 \uc57d 600~950 C(1110~1740 F)\uc5d0\uc11c \ud615\uc131\ub418\uace0 M7C3\ub294 \uadf8 \uc774\uc0c1\uc5d0\uc11c \ud615\uc131\ub418\ubbc0\ub85c, \uc774 \uc601\uc5ed\uc758 \ubaa8\ub4e0 \ud15c\ud37c\ub9c1 \uc2a4\ucf00\uc904\uc740 \uc815\uc758\uc0c1 \ud0c4\ud654\ubb3c \uc11d\ucd9c \uc2a4\ucf00\uc904\uc774\ub2e4. \ub610\ud55c \ucd9c\ucc98\ub294 \uc9c8\uc18c\uac00 \uace0\ud569\uae08 \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uac15\uc885\uc744 \uc6a9\uc811 \uc0c1\ud0dc \uadf8\ub300\ub85c \uc0ac\uc6a9\ud560 \uc218 \uc788\uac8c \ud558\ub294 \uc774\uc720\ub97c \uba85\ud655\ud788 \ubc1d\ud788\uace0 \uc788\ub294\ub370, \uc9c8\uc18c\uac00 \uae08\uc18d\uac04 \ud654\ud569\ubb3c \uc0c1\uc758 \uc11d\ucd9c\uc744 \uc9c0\uc5f0\uc2dc\ud0a4\uae30 \ub54c\ubb38\uc774\ub2e4. \ud2f0\ud0c0\ub284\uc774\ub098 \ub2c8\uc624\ube00\uc73c\ub85c \uc548\uc815\ud654\ub41c \uac15\uc885\uc5d0\uc11c\ub294 \uc57d 815 C(1500 F) \uc774\uc0c1\uc5d0\uc11c \uc774\ub4e4 \uc6d0\uc18c\uac00 \ud06c\ub86c\ubcf4\ub2e4 \ub354 \uc548\uc815\ud55c \ud0c4\ud654\ubb3c\uc744 \ud615\uc131\ud558\ubbc0\ub85c \ud06c\ub86c \ud0c4\ud654\ubb3c \ubb38\uc81c\uac00 \ub300\ubd80\ubd84 \ud574\uc18c\ub41c\ub2e4. \uc5ec\uae30\uc5d0\ub294 \ud55c \uac00\uc9c0 \ub2e8\uc11c\uac00 \ub530\ub974\uba70, \ucd9c\ucc98\ub294 \uc774\ub97c \uc9c1\uc811 \uba85\uc2dc\ud558\uace0 \uc788\ub2e4. \ud2f0\ud0c0\ub284 \ud0c4\ud654\ubb3c \uc790\uccb4\uac00 \uc9c8\uc0b0\uc5d0 \uc758\ud574 \uacf5\uaca9\ubc1b\uc744 \uc218 \uc788\uc73c\ubbc0\ub85c, \ud2f0\ud0c0\ub284 \uc548\uc815\ud654 \uac15\uc774 \uace0\uc0b0\ud654\uc131 \ub9e4\uccb4\uc5d0\uc11c \uc790\ub3d9\uc73c\ub85c \uc815\ub2f5\uc774 \ub418\ub294 \uac83\uc740 \uc544\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc2dc\uadf8\ub9c8 \uc0c1\uc774 \ubd80\uc2dd \uc18d\ub3c4\uc5d0 \ubbf8\uce58\ub294 \ube44\uc6a9<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98\uc758 \ud55c \uce21\uc815 \uc138\ud2b8\ub294 \uc5b4\ub5a4 \uc124\uba85\ubcf4\ub2e4\ub3c4 \uc774 \uc810\uc744 \uc798 \ubcf4\uc5ec\uc900\ub2e4. \ub2e8\uc77c Fe-47Cr \ud569\uae08\uc744 \uc5f4\ucc98\ub9ac\ud558\uc5ec \uc804\ubd80 \ud398\ub77c\uc774\ud2b8\uc774\uac70\ub098 \uc804\ubd80 \uc2dc\uadf8\ub9c8 \uc0c1\uc774 \ub418\ub3c4\ub85d \ud558\uace0, \ub450 \uc870\uc9c1\uc744 \ub3d9\uc77c\ud55c \uc6a9\uc561\uc5d0\uc11c \ub098\ub780\ud788 \uc2dc\ud5d8\ud558\uc600\ub2e4. \uc544\ub798 \ud45c\ub294 \ub450 \uc18d\ub3c4\uc640 \ucd9c\ucc98 \uc790\uccb4\uac00 \ubcf4\uace0\ud55c \ube44\uc728\uc744 \uc81c\uc2dc\ud55c\ub2e4. \ud658\uc6d0 \uc870\uac74\uc5d0\uc11c \uc2dc\uadf8\ub9c8 \uc0c1\uc740 \ud398\ub77c\uc774\ud2b8\ubcf4\ub2e4 2~5\ubc30 \ube60\ub974\uac8c \ubd80\uc2dd\ub41c\ub2e4. \uc0b0\ud654 \uc870\uac74\uc5d0\uc11c\ub294 \uc0b0\uc5d0 \ub530\ub77c \ube44\uc728\uc774 10, 24, 42\ub85c \uc99d\uac00\ud558\uba70, \uc5fc\ud654\uc81c\uc774\ucca0 \uacf5\uc2dd \uc2dc\ud5d8\uc5d0\uc11c \ud398\ub77c\uc774\ud2b8\ub294 \uc804\ud600 \ubd80\uc2dd\ub418\uc9c0 \uc54a\ub294 \ubc18\uba74 \uc2dc\uadf8\ub9c8 \uc0c1\uc740 2.5 g\/dm2\/d\ub97c \uc783\ub294\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">Solution<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud398\ub77c\uc774\ud2b8, g\/dm2\/d<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc2dc\uadf8\ub9c8 \uc0c1, g\/dm2\/d<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ube44\uc728<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"4\">\ud658\uc6d0 \uc870\uac74<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10% HCl, \ube44\ub4f1<\/td><td class=\"has-text-align-left\" data-align=\"left\">1461<\/td><td class=\"has-text-align-left\" data-align=\"left\">7543<\/td><td class=\"has-text-align-left\" data-align=\"left\">5.2<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10% H2SO4, \ube44\ub4f1<\/td><td class=\"has-text-align-left\" data-align=\"left\">2939<\/td><td class=\"has-text-align-left\" data-align=\"left\">7422<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50% H2SO4, \ube44\ub4f1<\/td><td class=\"has-text-align-left\" data-align=\"left\">5088<\/td><td class=\"has-text-align-left\" data-align=\"left\">5280<\/td><td class=\"has-text-align-left\" data-align=\"left\">1.04<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"4\">\uc0b0\ud654 \uc870\uac74<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50% H2SO4 + Fe2(SO4)3, \ube44\ub4f1<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0195<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.196<\/td><td class=\"has-text-align-left\" data-align=\"left\">10<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">50% H2SO4 + CuSO4, \ube44\ub4f1<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0170<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.415<\/td><td class=\"has-text-align-left\" data-align=\"left\">24<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">65% HNO3, \ube44\ub4f1<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.0205<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.861<\/td><td class=\"has-text-align-left\" data-align=\"left\">42<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">HNO3 + HF, 65 C(150 F)<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.06<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\" colspan=\"4\">\uacf5\uc2dd \uc870\uac74<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">10% FeCl3.6H2O, \uc2e4\uc628<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.00<\/td><td class=\"has-text-align-left\" data-align=\"left\">2.5<\/td><td class=\"has-text-align-left\" data-align=\"left\">&#8230;<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ub3d9\uc77c\ud55c Fe-47Cr \ud569\uae08\uc5d0\uc11c \ud398\ub77c\uc774\ud2b8\uc758 \ubd80\uc2dd \uc18d\ub3c4\uc5d0 \ub300\ud55c \uc2dc\uadf8\ub9c8 \uc0c1\uc758 \ubd80\uc2dd \uc18d\ub3c4, 8\uac00\uc9c0 \uc6a9\uc561\uacfc 1\uac00\uc9c0 \uacf5\uc2dd \uc2dc\ud5d8. \ube44\uc728 \uc5f4\uc740 \ucd9c\ucc98 \uc790\uccb4\uc758 \uac12\uc774\ub2e4. \ucd9c\ucc98: \ud574\ub2f9 \ub17c\ubb38\uc758 Table 4.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98\ub294 \uc774\ub85c\ubd80\ud130 \ud558\ub098\uc758 \uacb0\ub860\uc744 \ub3c4\ucd9c\ud558\ub294\ub370, \uc774\ub294 \uc9c1\uad00\uc801\uc774\uc9c0 \uc54a\uc73c\ubbc0\ub85c \ubc18\ubcf5\ud560 \uac00\uce58\uac00 \uc788\ub2e4. \uc2dc\uadf8\ub9c8 \uc0c1\uc774 \ub0b4\uc2dd\uc131\uc744 \uc800\ud558\uc2dc\ud0a4\ub294 \uc774\uc720\ub97c \uc124\uba85\ud558\ub294 \ub370 \ud06c\ub86c \uacb0\ud54d \uba54\ucee4\ub2c8\uc998\uc740 \ud544\uc694\ud558\uc9c0 \uc54a\ub2e4. \uadf8\uac83\uc740 \ub2e8\uc21c\ud788 \ud398\ub77c\uc774\ud2b8\ubcf4\ub2e4 \uadf8 \uc790\uccb4\ub85c \ub354 \ube60\ub974\uac8c \ubd80\uc2dd\ub418\ub294 \uc870\uc9c1\uc774\ub2e4. \uc774\ub294 \uc2e4\ubb34\uc801 \uc9c8\ubb38\uc744 \ubc14\uafbc\ub2e4. \uc785\uacc4\uc758 \uc81c2\uc0c1 \ub124\ud2b8\uc6cc\ud06c\ub294 \ub35c \ub0b4\uc2dd\uc131\uc778 \uc7ac\ub8cc\uc758 \uc5f0\uc18d \uacbd\ub85c\uc774\uae30 \ub54c\ubb38\uc5d0 \ubb38\uc81c\uc774\uba70, \ub3d9\uc77c\ud55c \uc0c1\uc758 \uace0\ub9bd\ub41c \uc9d1\ud569\uccb4\ub294 \ubb38\uc81c\uac00 \ud6e8\uc52c \uc801\uc73c\ubbc0\ub85c, \ud615\uc131\ub41c \uac83\uc758 \uc591\ub9cc\ud07c\uc774\ub098 \ud615\uc131\ub41c \uac83\uc758 \ud615\ud0dc\uac00 \uc911\uc694\ud560 \uc218 \uc788\ub2e4. \ub0c9\uac04 \uac00\uacf5\uc740 \uc2dc\uadf8\ub9c8 \uc0c1\uc758 \uc11d\ucd9c\uc744 \uac00\uc18d\ud558\uba70, \uc57d 2%\uae4c\uc9c0\uc758 \ub2c8\ucf08 \ucca8\uac00\ub294 \uc774\ub97c \ub354\uc6b1 \uac00\uc18d\ud558\ub294 \ubc18\uba74 \ub354 \ub192\uc740 \ub2c8\ucf08 \uc218\uc900\uc740 \ub2e4\uc2dc \ub290\ub9ac\uac8c \ud55c\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ubbfc\uac10\ud654 \uc2dc\ud5d8 \ubc0f \ud569\uaca9 \uae30\uc900<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774\ub4e4 \uc2dc\ud5d8\uc758 \ubaa9\uc801\uc740 \uc0ac\uc6a9 \ud658\uacbd\uc744 \uc7ac\ud604\ud558\ub294 \uac83\uc774 \uc544\ub2c8\ub2e4. \uadf8\uac83\uc740 \uacf5\uae09\ub41c \uc7ac\ub8cc\uac00 \uc8fc\ubb38\ub41c \uc57c\uae08\ud559\uc801 \uc0c1\ud0dc\uc5d0 \uc788\ub294\uc9c0\ub77c\ub294 \ub354 \uc881\uc740 \uc9c8\ubb38\uc5d0 \ub2f5\ud558\ub294 \uac83\uc774\uba70, \uadf8\ub798\uc11c \uc774\ub4e4\uc774 \uc124\uacc4 \ub370\uc774\ud130\uac00 \uc544\ub2c8\ub77c \ud569\uaca9 \uc2dc\ud5d8\uc73c\ub85c \uc0ac\uc6a9\ub41c\ub2e4. \uc624\uc2a4\ud14c\ub098\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc758 \uacbd\uc6b0 \ud45c\uc900\uc740 ASTM A 262\uc774\uba70, \uc5ec\uae30\uc5d0\ub294 6\uac00\uc9c0 \uc2e4\ubb34 \ubc29\ubc95\uc774 \ud3ec\ud568\ub41c\ub2e4. Practice A\ub294 \uc804\ud574 \uc625\uc0b4\uc0b0 \uc5d0\uce6d\uc73c\ub85c, \uc218 \ubd84\uc774 \uac78\ub9ac\ub294 \uc2a4\ud06c\ub9ac\ub2dd \uc2dc\ud5d8\uc774\uba70 \uc5d0\uce6d\ub41c \ubbf8\uc138\uc870\uc9c1\uc744 \uac80\uc0ac\ud558\uc5ec \ud06c\ub86c \ud0c4\ud654\ubb3c \ubbfc\uac10\ud654\ub97c \ud310\uc815\ud55c\ub2e4. Practice B\ub294 \ube44\ub4f1 \uc5fc\ud654\uc81c\uc774\ucca0 + \ud669\uc0b0\uc5d0\uc11c 120\uc2dc\uac04\uc744 \uc9c4\ud589\ud558\uace0 \uc911\ub7c9 \uac10\uc18c\uc728\uc744 \ubcf4\uace0\ud55c\ub2e4. Practice C\ub294 \ube44\ub4f1 65% \uc9c8\uc0b0\uc5d0\uc11c 240\uc2dc\uac04\uc744 \uc9c4\ud589\ud558\uba70 \ud0c4\ud654\ubb3c\ubfd0 \uc544\ub2c8\ub77c \uc2dc\uadf8\ub9c8 \uc0c1\ub3c4 \uac80\ucd9c\ud55c\ub2e4. Practice E\ub294 \uae08\uc18d \uad6c\ub9ac\ub97c \ucca8\uac00\ud55c \ube44\ub4f1 6% \ud669\uc0b0\uad6c\ub9ac + 10% \ud669\uc0b0\uc5d0\uc11c 24\uc2dc\uac04\uc744 \uc9c4\ud589\ud558\uba70, \uc2dc\ud3b8\uc744 \uad7d\ud600 \uade0\uc5f4\uc744 \ucc3e\uc544 \ud310\uc815\ud55c\ub2e4. Practice F\ub294 \uad6c\ub9ac\uac00 \uc874\uc7ac\ud558\ub294 \ud669\uc0b0\uad6c\ub9ac + 50% \ud669\uc0b0\uc5d0\uc11c 120\uc2dc\uac04 \ube44\ub4f1 \uc2dc\ud5d8\uc774\uba70, \ubab0\ub9ac\ube0c\ub374 \ud568\uc720 \uac15\uc885\uc744 \ub300\uc0c1\uc73c\ub85c \ud55c\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud398\ub77c\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc740 ASTM A 763\uc73c\ub85c \ucc98\ub9ac\ub418\uba70, \uc774\ub294 \uc625\uc0b4\uc0b0 \uc5d0\uce6d\uacfc 3\uac00\uc9c0 \uc0b0 \uce68\uc9c0 \uc2dc\ud5d8\uc73c\ub85c A 262\uc640 \uac19\uc740 \ud615\ud0dc\ub97c \ub530\ub978\ub2e4. \uac00\uacf5\ub41c \ub2c8\ucf08 \ubd80\ud654 \ud06c\ub86c \ud569\uae08\uc740 ASTM G 28\ub85c \ucc98\ub9ac\ub41c\ub2e4. A 763\uc758 \ud55c \uac00\uc9c0 \uad6c\uc870\uc801 \ucc28\uc774\ub294 \uc0b0 \ub178\ucd9c\uc774 \ud604\ubbf8\uacbd\ud558\uc5d0\uc11c \ud310\uc815\ub418\uba70, \uc785\uacc4 \ub099\ud558(grain dropping)\uc758 \uc720\ubb34\uac00 \ud569\uaca9 \uae30\uc900\uc774 \ub41c\ub2e4\ub294 \uc810\uc774\ub2e4. \uc544\ub798 \ud45c\ub294 \ucd9c\ucc98\uac00 \ud45c\ub85c \uc815\ub9ac\ud55c \ud569\uaca9 \uae30\uc900\uc744 \uc218\uc9d1\ud55c \uac83\uc73c\ub85c, \uba3c\uc800 \uc801\uc6a9\ub418\ub294 \ubbfc\uac10\ud654 \ucc98\ub9ac\ub97c \ud3ec\ud568\ud55c\ub2e4. \uc65c\ub0d0\ud558\uba74 \uadf8\uac83\uc744 \uc0dd\uc131\ud55c \ucc98\ub9ac \uc5c6\uc774 \ud55c\uacc4\uac12\ub9cc\uc73c\ub85c\ub294 \uc0ac\uc6a9 \uac00\ub2a5\ud55c \uaddc\uaca9\uc774 \ub418\uc9c0 \uc54a\uae30 \ub54c\ubb38\uc774\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ud569\uae08<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubbfc\uac10\ud654 \ucc98\ub9ac<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc2dc\ud5d8<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ub178\ucd9c, h<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ucd5c\ub300 \ud5c8\uc6a9 \uc18d\ub3c4, mm\/month (mils\/month)<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">Type 304<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5c6\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5fc\ud654\uc81c\uc774\ucca0, A 262-B<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.1 (4)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Type 304L<\/td><td class=\"has-text-align-left\" data-align=\"left\">675 C(1250 F)\uc5d0\uc11c 1 h<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc9c8\uc0b0, A 262-C<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 (2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Type 309S<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5c6\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc9c8\uc0b0, A 262-C<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.025 (1)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Type 316<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5c6\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5fc\ud654\uc81c\uc774\ucca0, A 262-B<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.1 (4)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Type 316L<\/td><td class=\"has-text-align-left\" data-align=\"left\">675 C(1250 F)\uc5d0\uc11c 1 h<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5fc\ud654\uc81c\uc774\ucca0, A 262-B<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.1 (4)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Type 317L<\/td><td class=\"has-text-align-left\" data-align=\"left\">675 C(1250 F)\uc5d0\uc11c 1 h<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5fc\ud654\uc81c\uc774\ucca0, A 262-B<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.1 (4)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Type 321<\/td><td class=\"has-text-align-left\" data-align=\"left\">675 C(1250 F)\uc5d0\uc11c 1 h<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc9c8\uc0b0, A 262-C<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 (2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Type 347<\/td><td class=\"has-text-align-left\" data-align=\"left\">675 C(1250 F)\uc5d0\uc11c 1 h<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc9c8\uc0b0, A 262-C<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 (2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">20Cb-3<\/td><td class=\"has-text-align-left\" data-align=\"left\">675 C(1250 F)\uc5d0\uc11c 1 h<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud669\uc0b0\uc81c\uc774\ucca0, G 28-A<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 (2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">904L<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5c6\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud669\uc0b0\uc81c\uc774\ucca0, G 28-A<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.05 (2)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">Incoloy 825<\/td><td class=\"has-text-align-left\" data-align=\"left\">675 C(1250 F)\uc5d0\uc11c 1 h<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc9c8\uc0b0, A 262-C<\/td><td class=\"has-text-align-left\" data-align=\"left\">240<\/td><td class=\"has-text-align-left\" data-align=\"left\">0.075 (3)<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">29-4-2<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5c6\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud669\uc0b0\uc81c\uc774\ucca0, A 763-X<\/td><td class=\"has-text-align-left\" data-align=\"left\">120<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc720\uc758\ubbf8\ud55c \uc785\uacc4 \ud0c8\ub77d \uc5c6\uc74c<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98\uac00 \ud45c\ub85c \uc81c\uc2dc\ud55c \uc804\uc2e0 \ud569\uae08\uc758 \ud3c9\uac00 \uc2dc\ud5d8 \ubc0f \ud569\uaca9 \uae30\uc900\uc73c\ub85c, \uac01\uac01\uc5d0 \ub300\ud55c \uc801\uaca9 \uac10\uc218\ud654 \ucc98\ub9ac\uc640 \ud569\uaca9 \ud55c\uacc4\ub97c \ud3ec\ud568\ud55c\ub2e4. \ucd9c\ucc98: Evaluating Intergranular Corrosion \ub17c\ubb38\uc758 Table 1.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc778\uc99d \uc2dc\ub8cc\uac00 \uc544\ub2cc \ub2e8\uc77c \uc0dd\uc0b0 \ubd80\ud488\uc744 \uac80\uc0ac\ud558\ub294 \uacbd\uc6b0, \ucd9c\ucc98\ub294 ASTM G 108\uc758 \uc804\uae30\ud654\ud559\uc801 \uc7ac\ud65c\uc131\ud654 \uc2dc\ud5d8\uc744 \uc124\uba85\ud55c\ub2e4. \uc5f0\ub9c8\ub41c \uc2dc\ud3b8\uc744 \ud669\uc0b0\uacfc \ud2f0\uc624\uc2dc\uc548\uc0b0\uce7c\ub968 \uc6a9\uc561\uc5d0\uc11c \ubd80\ub3d9\ud0dc \uc0c1\ud0dc\ub85c\ubd80\ud130 \ud65c\uc131 \uc601\uc5ed\uc73c\ub85c \ubd84\uadf9\uc2dc\ud0a4\uace0, \uc7ac\ud65c\uc131\ud654 \ub3d9\uc548 \ud1b5\uacfc\ud55c \uc804\ud558\ub7c9\uc744 \uc785\uacc4\uc758 \ud06c\ub86c \ud0c4\ud654\ubb3c \uc11d\ucd9c\uacfc \uc5f0\uad00\uc2dc\ud0a8\ub2e4. \ucd9c\ucc98\uac00 \uc81c\uc2dc\ud558\ub294 \uae30\uc900\uac12\uc740 \ubbf8\uac10\uc218\ud654 \uc870\uc9c1\uc758 \uacbd\uc6b0 \ub2e8\uc704 \uc785\uacc4 \uba74\uc801\ub2f9 \uc804\ud558\ub7c9 0.1 C\/cm2 \ubbf8\ub9cc, \uc2ec\ud558\uac8c \uac10\uc218\ud654\ub41c \uc870\uc9c1\uc758 \uacbd\uc6b0 0.4 C\/cm2 \ucd08\uacfc\uc774\ub2e4. \uc774 \uc2dc\ud5d8\uc740 120\uc2dc\uac04 \ubc0f 240\uc2dc\uac04 \uc0b0 \uce68\uc9c0 \uc2dc\ud5d8\uacfc \ub2ec\ub9ac, \uc5f4\ucc98\ub9ac \ub85c\ud2b8\uc5d0\uc11c \ucc44\ucde8\ud55c \ubd80\ud488\uc5d0 \uc801\uc6a9\ud560 \uc218 \uc788\uc744 \ub9cc\ud07c \ube60\ub974\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uacf5\uad6c\uac15 \uc8fc\ubb38\uc5d0\uc11c \uc774\uac83\uc774 \uc758\ubbf8\ud558\ub294 \ubc14<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc2a4\ud14c\uc778\ub9ac\uc2a4 \uacf5\uad6c\uac15\uc744 \uad6c\ub9e4\ud558\uac70\ub098 \uc5f4\ucc98\ub9ac\ud558\ub294 \uc0ac\ub78c\uc5d0\uac8c \uc774\ub85c\ubd80\ud130 \uc138 \uac00\uc9c0\uac00 \ub530\ub978\ub2e4. \ud654\ud559 \uc870\uc131\uacfc \uc5f4\ucc98\ub9ac\uac00 \ud568\uaed8 \ub0b4\uc2dd\uc131\uc744 \uacb0\uc815\ud558\ubbc0\ub85c, \ubd80\ud488\uc744 \ud15c\ud37c\ub9c1\ud558\uac70\ub098 \uc751\ub825 \uc81c\uac70\ud560 \uacbd\uc6b0 \ubd84\uc11d\ub9cc\uc73c\ub85c \uac15\uc885\uc744 \uc120\ud0dd\ud574\uc11c\ub294 \uc548 \ub41c\ub2e4. \uc704 \ud45c\uc758 \uc774\ucc28 \uc0c1\ub4e4\uc740 \ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uac15\uc885\uc758 \ud15c\ud37c\ub9c1 \ubc94\uc704\uc640 \uacb9\uce58\ubbc0\ub85c, \ud15c\ud37c\ub9c1 \uc628\ub3c4\ub294 \uacbd\ub3c4\uc640 \ub0b4\uc2dd\uc131 \uc694\uad6c \uc0ac\ud56d \ubaa8\ub450\ub97c \uace0\ub824\ud558\uc5ec \uc120\ud0dd\ud574\uc57c \ud55c\ub2e4. \uadf8\ub9ac\uace0 \uac10\uc218\ud654\uac00 \ubb38\uc81c\ub418\ub294 \uacbd\uc6b0, \ud569\uaca9 \uc2dc\ud5d8\uc740 \uc801\uaca9 \uac10\uc218\ud654 \ucc98\ub9ac\uc640 \ud568\uaed8 \uad6c\ub9e4 \uc0ac\uc591\uc11c\uc5d0 \ud3ec\ud568\ub418\uc5b4\uc57c \ud558\ub294\ub370, \ud55c\uacc4\uac12\ub9cc\uc73c\ub85c\ub294 \uc544\ubb34\uac83\ub3c4 \uc124\uba85\ud558\uc9c0 \ubabb\ud558\uae30 \ub54c\ubb38\uc774\ub2e4. \uc5f4\ucc98\ub9ac \uce21\uba74\uc5d0\uc11c \ub3d9\uc77c\ud55c \uc57c\uae08\ud559\uc801 \uadf8\ub9bc\uc740 \ub2e4\uc74c\uc5d0 \uc788\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/martensitic-stainless-steel-microstructure\/\">\ub9c8\ub974\ud150\uc0ac\uc774\ud2b8\uacc4 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15\uc758 \ubbf8\uc138\uc870\uc9c1<\/a>, \uc0ac\uc774\ud074 \uc790\uccb4\ub294 \ub2e4\uc74c\uc5d0 \uc788\uc73c\uba70 <a href=\"https:\/\/aobosteel.com\/ko\/440c-stainless-steel-heat-treatment\/\">440C \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \uc5f4\ucc98\ub9ac<\/a> \uadf8\ub9ac\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/420-stainless-steel-heat-treatment\/\">420 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \uc5f4\ucc98\ub9ac<\/a>, Aobo\uac00 \uacf5\uae09\ud558\ub294 \uac15\uc885\uc758 \ubd80\uc2dd \uac70\ub3d9\uc740 \ub2e4\uc74c\uc5d0 \ub3c4\ud45c\ub85c \uc81c\uc2dc\ub418\uc5b4 \uc788\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/stainless-steel-corrosion-resistance-chart\/\">\uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \ub0b4\uc2dd\uc131 \ucc28\ud2b8<\/a>. \uc798\ubabb\ub41c \uc5f4\ucc98\ub9ac\ub85c \uc778\ud55c \uc0ac\uc6a9 \uc911 \ud30c\uc190\uc740 \ub2e4\uc74c\uc5d0 \uc788\uc73c\uba70 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-size-change-in-heat-treatment\/\">\uc5f4\ucc98\ub9ac \uc2dc \uce58\uc218 \ubcc0\ud654<\/a> \uadf8\ub9ac\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/quench-cracking-tool-steel\/\">\uacf5\uad6c\uac15\uc758 \ub2f4\uae08\uc9c8 \uade0\uc5f4<\/a>, \ub3d9\uc77c\ud55c \uc785\uacc4 \ubb38\uc81c\uc758 \uccad\uc815\ub3c4 \uce21\uba74\uc740 \ub2e4\uc74c\uc5d0 \uc788\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/steel-inclusion-and-grain-size-measurement\/\">\uac1c\uc7ac\ubb3c \ubc0f \uacb0\uc815\ub9bd \ud06c\uae30 \uce21\uc815<\/a> \ubc0f <a href=\"https:\/\/aobosteel.com\/ko\/steel-bar-and-billet-inspection\/\">\uac15\ubd09 \ubc0f \ube4c\ub9bf \uac80\uc0ac \ud398\uc774\uc9c0<\/a>, \uac15\uc885 \uc790\uccb4\ub294 \ub2e4\uc74c\uc5d0 \uc124\uba85\ub418\uc5b4 \uc788\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/4cr13-stainless-steel\/\">4Cr13 \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15<\/a> \uadf8\ub9ac\uace0 <a href=\"https:\/\/aobosteel.com\/ko\/plastic-mold-steels\/\">\ud50c\ub77c\uc2a4\ud2f1 \uae08\ud615\uac15<\/a>. \uc5fc\ud654\ubb3c \ud658\uacbd\uc774 \ud568\uaed8 \uc874\uc7ac\ud558\ub294 \uacbd\uc6b0 \uc785\uacc4 \uacf5\uaca9\uc774 \uade0\uc5f4\ub85c \ubc1c\uc804\ud560 \uc218 \uc788\uc73c\uba70, \uc774\ub294 \ub2e4\uc74c\uc758 \uc8fc\uc81c\uc774\ub2e4: <a href=\"https:\/\/aobosteel.com\/ko\/steel-embrittlement-types\/\">\uac15\uc758 \ucde8\ud654 \uc720\ud615<\/a>.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\uac10\uc218\ud654 \uc9c4\ub2e8\uc5d0 \ub530\ub77c \uc870\uce58\ud558\uae30 \uc804\uc5d0<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\ucc38\uace0 \uc790\ub8cc \ud398\uc774\uc9c0\uc774\uba70, Aobo Steel\uc758 \uc0ac\uc591\uc11c\uac00 \uc544\ub2c8\uace0, \uc704\uc758 \uc18d\ub3c4\uc640 \uae30\uc900\uc740 \uba85\uc2dc\ub41c \ud2b9\uc815 \ud569\uae08, \ucc98\ub9ac \ubc0f \uc6a9\uc561\uc5d0 \ub300\ud574 \ubc1c\ud45c\ub41c \uac12\uc774\ub2e4. \ucd09\uc9c4 \uc0b0 \uc2dc\ud5d8\uc740 \uc7ac\ub8cc\ub97c \ub4f1\uae09\ud654\ud558\uace0 \ub0a9\ud488 \uc0c1\ud0dc\ub97c \ud655\uc778\ud558\ub294 \uac83\uc774\uc9c0, \ud50c\ub79c\ud2b8\uc5d0\uc11c\uc758 \uc0ac\uc6a9 \uc218\uba85\uc744 \uc608\uce21\ud558\ub294 \uac83\uc774 \uc544\ub2c8\ub2e4. \uc628\ub3c4 \ubc94\uc704\ub294 \ucd9c\ucc98\uac00 \uc124\uba85\ud55c \uc2a4\ud14c\uc778\ub9ac\uc2a4\uac15 \uacc4\uc5f4\uc5d0 \ub300\ud574 \uc81c\uc2dc\ub41c \uac83\uc774\uba70, \uac10\uc218\ud654 \uad6c\uac04\uc758 \uc815\ud655\ud55c \uacbd\uacc4\ub294 \uc55e\uc5d0 \uc788\ub294 \uac15\uc885\uc758 \ud0c4\uc18c \ud568\ub7c9, \uc9c8\uc18c \ud568\ub7c9 \ubc0f \uc548\uc815\ud654 \ucca8\uac00 \uc6d0\uc18c\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9c4\ub2e4. \ud569\uaca9 \ud55c\uacc4\ub294 \uc790\uccb4\uc801\uc778 \uc801\uaca9 \ucc98\ub9ac \uc870\uac74\uc744 \uba85\uc2dc\ud55c \uad6c\ub9e4 \uc0ac\uc591\uc11c\uc758 \ucd9c\ubc1c\uc810\uc73c\ub85c \uc0bc\uace0, \uc5f4\ucc98\ub9ac\uc5d0 \uacb0\ud568\uc774 \uc788\ub2e4\uace0 \uacb0\ub860 \ub0b4\ub9ac\uae30 \uc804\uc5d0 \uc2e4\uc81c \ubd80\ud488\uc758 \uc870\uc9c1\uc744 \ud655\uc778\ud558\ub77c.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Volume 13A, Corrosion: Fundamentals, Testing, and Protection, ASM International, 2003.<\/p>","protected":false},"excerpt":{"rendered":"<p>Sensitization and Intergranular Corrosion in Stainless Tool Steel A stainless tool steel that failed along its grain boundaries usually passed every check on the drawing. The grade is right, the hardness is right, and the surface was clean. What went wrong is a heat treatment step that walked the steel through one temperature range, or [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-21191","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Sensitization and Intergranular Corrosion in Stainless Tool Steel<\/title>\n<meta name=\"description\" content=\"Chromium carbide precipitation between 425 and 815 C leaves stainless tool steel sensitized at its grain boundaries. Mechanism, secondary phases and acceptance tests.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/stainless-steel-sensitization\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Sensitization and Intergranular Corrosion in Stainless Tool Steel\" \/>\n<meta property=\"og:description\" content=\"Chromium carbide precipitation between 425 and 815 C leaves stainless tool steel sensitized at its grain boundaries. Mechanism, secondary phases and acceptance tests.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/stainless-steel-sensitization\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-11-12T12:16:33+00:00\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"13\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Sensitization and Intergranular Corrosion in Stainless Tool Steel\",\"datePublished\":\"2026-10-07T13:21:52+00:00\",\"dateModified\":\"2026-11-12T12:16:33+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/\"},\"wordCount\":2641,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/\",\"name\":\"Sensitization and Intergranular Corrosion in Stainless Tool Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"datePublished\":\"2026-10-07T13:21:52+00:00\",\"dateModified\":\"2026-11-12T12:16:33+00:00\",\"description\":\"Chromium carbide precipitation between 425 and 815 C leaves stainless tool steel sensitized at its grain boundaries. Mechanism, secondary phases and acceptance tests.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/stainless-steel-sensitization\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Sensitization and Intergranular Corrosion in Stainless Tool Steel\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\uc2a4\ud14c\uc778\ub9ac\uc2a4 \uacf5\uad6c\uac15\uc758 \uc608\ubbfc\ud654 \ubc0f \uc785\uacc4 \ubd80\uc2dd","description":"425~815 C \uc0ac\uc774\uc758 \ud06c\ub86c \ud0c4\ud654\ubb3c \uc11d\ucd9c\uc740 \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uacf5\uad6c\uac15\uc758 \uc785\uacc4\ub97c \uc608\ubbfc\ud654\uc2dc\ud0b5\ub2c8\ub2e4. \uba54\ucee4\ub2c8\uc998, \uc774\ucc28 \uc0c1, \ud569\uaca9 \uc2dc\ud5d8\uc785\ub2c8\ub2e4.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/stainless-steel-sensitization\/","og_locale":"ko_KR","og_type":"article","og_title":"Sensitization and Intergranular Corrosion in Stainless Tool Steel","og_description":"Chromium carbide precipitation between 425 and 815 C leaves stainless tool steel sensitized at its grain boundaries. Mechanism, secondary phases and acceptance tests.","og_url":"https:\/\/aobosteel.com\/ko\/stainless-steel-sensitization\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-11-12T12:16:33+00:00","twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"13\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Sensitization and Intergranular Corrosion in Stainless Tool Steel","datePublished":"2026-10-07T13:21:52+00:00","dateModified":"2026-11-12T12:16:33+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/"},"wordCount":2641,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/","url":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/","name":"\uc2a4\ud14c\uc778\ub9ac\uc2a4 \uacf5\uad6c\uac15\uc758 \uc608\ubbfc\ud654 \ubc0f \uc785\uacc4 \ubd80\uc2dd","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"datePublished":"2026-10-07T13:21:52+00:00","dateModified":"2026-11-12T12:16:33+00:00","description":"425~815 C \uc0ac\uc774\uc758 \ud06c\ub86c \ud0c4\ud654\ubb3c \uc11d\ucd9c\uc740 \uc2a4\ud14c\uc778\ub9ac\uc2a4 \uacf5\uad6c\uac15\uc758 \uc785\uacc4\ub97c \uc608\ubbfc\ud654\uc2dc\ud0b5\ub2c8\ub2e4. \uba54\ucee4\ub2c8\uc998, \uc774\ucc28 \uc0c1, \ud569\uaca9 \uc2dc\ud5d8\uc785\ub2c8\ub2e4.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/stainless-steel-sensitization\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/stainless-steel-sensitization\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Sensitization and Intergranular Corrosion in Stainless Tool Steel"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Sensitization and Intergranular Corrosion in Stainless Tool Steel A stainless tool steel that failed along its grain boundaries usually passed every check on the drawing. The grade is right, the hardness is right, and the surface was clean. What went wrong is a heat treatment step that walked the steel through one temperature range, or&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Sensitization and Intergranular Corrosion in Stainless Tool Steel A stainless tool steel that failed along its grain boundaries usually passed every check on the drawing. The grade is right, the hardness is right, and the surface was clean. What went wrong is a heat treatment step that walked the steel through one temperature range, or&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21191","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=21191"}],"version-history":[{"count":4,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21191\/revisions"}],"predecessor-version":[{"id":25300,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21191\/revisions\/25300"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=21191"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}