{"id":21170,"date":"2026-10-07T20:19:01","date_gmt":"2026-10-07T12:19:01","guid":{"rendered":"https:\/\/aobosteel.com\/?page_id=21170"},"modified":"2026-10-16T01:40:54","modified_gmt":"2026-10-15T17:40:54","slug":"tool-steel-fatigue-failure","status":"publish","type":"page","link":"https:\/\/aobosteel.com\/ko\/tool-steel-fatigue-failure\/","title":{"rendered":"\uacf5\uad6c\uac15\uc758 \ud53c\ub85c \ud30c\uad34"},"content":{"rendered":"<h1 class=\"wp-block-heading\">\uacf5\uad6c\uac15\uc758 \ud53c\ub85c \ud30c\uad34<\/h1>\n\n\n\n<p class=\"wp-block-paragraph\">\ud53c\ub85c\ub85c \ud30c\uad34\ub41c \uacf5\uad6c\ub294 \ub3c4\uba74\uc774 \uc694\uad6c\ud55c \uac80\uc0ac\ub97c \ud1b5\uacfc\ud55c \uac83\uc785\ub2c8\ub2e4. \uacbd\ub3c4\ub294 \uaddc\uaca9\uc5d0 \ub9de\uace0, \uac15\uc885\uc740 \uc6a9\ub3c4\uac00 \uc694\uad6c\ud55c \uac83\uc774\uba70, \ud558\uc911\uc740 \uc124\uacc4 \uac12\uc744 \ucd08\uacfc\ud55c \uc801\uc774 \uc5c6\uc2b5\ub2c8\ub2e4. \uadf8\ub7f0\ub370\ub3c4 \uade0\uc5f4\uc740 \uc2dc\uc791\ub418\uc5c8\uace0, \ub300\uac1c \uc544\ubb34\ub3c4 \uc9c0\uc815\ud558\uc9c0 \uc54a\uc740 \ud615\uc0c1\uc5d0\uc11c \uc2dc\uc791\ub418\uc5b4 \ub9e4 \uc0ac\uc774\ud074\ub9c8\ub2e4 \uc870\uae08\uc529 \uc131\uc7a5\ud558\ub2e4\uac00 \ub0a8\uc740 \ub2e8\uba74\uc774 \ud30c\ub2e8\ub418\uc5c8\uc2b5\ub2c8\ub2e4. \uc774 \ud398\uc774\uc9c0\uc5d0\uc11c\ub294 \uacf5\uad6c\uc5d0\uc11c \ud53c\ub85c \uade0\uc5f4\uc774 \uc2dc\uc791\ub418\ub294 \uc704\uce58, \uc774\ub97c \uacb0\uc815\ud558\ub294 \ub9c8\ud0b9 \ubc0f \ub9c8\ubb34\ub9ac \uad00\ud589, \ub864\uc774\ub098 \uae30\uc5b4 \uc774\ube68\uc744 \uc0ac\uc6a9 \ubd88\ub2a5\uc73c\ub85c \ub9cc\ub4dc\ub294 \uc811\ucd09 \ud53c\ub85c \ubaa8\ub4dc, \uadf8\ub9ac\uace0 \uad00\ub828\ub41c \ub450 \uc0b0\uc5c5\uc774 \uac01\uac01\uc744 \ubb34\uc5c7\uc73c\ub85c \ubd80\ub974\uae30\ub85c \ucd5c\uc885 \ud569\uc758\ud588\ub294\uc9c0\ub97c \ub2e4\ub8f9\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uc544\ubb34\ub3c4 \ubcf4\uc9c0 \uc54a\uc740 \uacf3\uc5d0\uc11c \ud53c\ub85c \uade0\uc5f4\uc774 \uc2dc\uc791\ub418\ub294 \uc774\uc720<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud53c\ub85c \ud30c\uad34\ub294 \uad6d\ubd80 \uc751\ub825\uc774 \ub2e8\uba74\uc758 \uacf5\uce6d \uc751\ub825\ubcf4\ub2e4 \ub192\uc740 \uacf3\uc5d0\uc11c \uc2dc\uc791\ub418\uba70, \ucd5c\ub300\uac12\uc774 \uac15\uc758 \ud56d\ubcf5 \uac15\ub3c4 \uc774\ud558\ub85c \uc720\uc9c0\ub418\ub294 \ubc18\ubcf5 \ud558\uc911 \ud558\uc5d0\uc11c \uc131\uc7a5\ud569\ub2c8\ub2e4. \uadf8 \uacb0\uacfc \ubc1c\uc0dd\ud558\ub294 \ud30c\ub2e8\uba74\uc740 \ub450 \uac1c\uc758 \uc601\uc5ed\uc744 \uac00\uc9c0\ub294\ub370, \uade0\uc5f4\uc774 \uc0ac\uc774\ud074\ub9c8\ub2e4 \uc9c4\ud589\ub41c \ub9e4\ub044\ub7ec\uc6b4 \uc810\uc9c4\uc801 \uc601\uc5ed\uacfc \ub0a8\uc740 \ub2e8\uba74\uc774 \ud30c\ub2e8\ub41c \ub354 \uac70\uce5c \ucd5c\uc885 \uc601\uc5ed\uc785\ub2c8\ub2e4. \ub2e8\uba74\uc5d0 \ub300\ud55c \uc810\uc9c4\uc801 \uc601\uc5ed\uc758 \ud06c\uae30\ub294 \ubd80\ud488\uc774 \uc2e4\uc81c\ub85c \ubc1b\uace0 \uc788\ub358 \ud558\uc911\uc758 \uc9c1\uc811\uc801\uc778 \ucc99\ub3c4\uc774\uba70, \uc774\uac83\uc774 \uc808\ub2e8 \uc804\uc5d0 \ub450 \uc601\uc5ed\uc744 \ucd2c\uc601\ud560 \uac00\uce58\uac00 \uc788\ub294 \uc774\uc720\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uae30\uc810\uc758 \uc704\uce58\ub294 \uacf5\uad6c \uc81c\uc791 \ud604\uc7a5\uc774 \uc870\uce58\ud560 \uc218 \uc788\ub294 \ubd84\uc11d \ubd80\ubd84\uc778\ub370, \uc774\ub294 \uac70\uc758 \ud56d\uc0c1 \ub204\uad70\uac00\uac00 \uac00\uacf5\ud55c \ud615\uc0c1\uc774\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \uae30\uacc4 \uac00\uacf5 \ud648, \uac01\uc778 \uc790\uad6d, \uc5f0\uc0ad \uace8, \ub0a0\uce74\ub85c\uc6b4 \ub0b4\ubd80 \ucf54\ub108, \uac1c\uc7ac\ubb3c, \ud0c8\ud0c4\uce35, \ubd80\uc2dd \ud53c\ud2b8\ub294 \ubaa8\ub450 \ub178\uce58\uc774\uba70, \ub178\uce58\ub294 \uae4a\uc774\uc640 \ubc18\uacbd\uc5d0 \uc758\ud574 \uacb0\uc815\ub418\ub294 \uacc4\uc218\ub9cc\ud07c \uacf5\uce6d \uc751\ub825\uc744 \uc99d\ud3ed\uc2dc\ud0b5\ub2c8\ub2e4. \uc544\ub798 \ud45c\ub294 \ucd9c\ucc98\uc5d0\uc11c \ub2e4\ub8e8\ub294 \ubd80\uc704\ub97c \ub098\uc5f4\ud558\uace0, \uac01 \ubd80\uc704\uac00 \uc560\ucd08\uc5d0 \uc874\uc7ac\ud574\uc57c \ud558\ub294\uc9c0\ub97c \uacb0\uc815\ud558\ub294 \uacf5\uc815 \uc810\uac80 \uc0ac\ud56d\uacfc \uc9dd\uc9c0\uc5b4 \ubcf4\uc5ec\uc90d\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uac1c\uc2dc \ubd80\uc704<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud574\ub2f9 \ubd80\uc704\uc5d0 \uc751\ub825\uc774 \uc9d1\uc911\ub418\ub294 \uc774\uc720<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uba3c\uc800 \uc810\uac80\ud560 \uc0ac\ud56d<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uae30\uacc4 \uac00\uacf5 \ub610\ub294 \uc5f0\uc0ad \ud648<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud648\uc740 \ub178\uce58\uc774\uba70, \ub178\uce58\ub294 \uae4a\uc774\uc640 \ubc18\uacbd\uc5d0 \uc758\ud574 \uacb0\uc815\ub418\ub294 \uacc4\uc218\ub9cc\ud07c \uacf5\uce6d \uc751\ub825\uc744 \uc99d\ud3ed\uc2dc\ud0b5\ub2c8\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub3c4\uba74\uc758 \ub9c8\ubb34\ub9ac \uc9c0\uc2dc \uc0ac\ud56d, \uadf8\ub9ac\uace0 \ucd5c\uc885 \uacf5\uc815\uc774 \uc6d0\uc8fc \ubc29\ud5a5 \uc790\uad6d\uc744 \ub0a8\uacbc\ub294\uc9c0 \uc5ec\ubd80<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc751\ub825\uc774 \uc791\uc6a9\ud558\ub294 \ubd80\uc704\uc758 \uc2dd\ubcc4 \uac01\uc778<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0c9\uac04 \uac01\uc778\uc740 \uae08\uc18d\uc744 \ubcc0\uc704\uc2dc\ud0a4\uace0 \ubb38\uc790 \uc724\uacfd \uc8fc\uc704\uc5d0 \ub178\uce58\ub97c \ub0a8\uae41\ub2c8\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc5f4 \ubc88\ud638\uc640 \ubd80\ud488 \ubc88\ud638\uac00 \uc801\uc6a9\ub41c \uc704\uce58, \uadf8\ub9ac\uace0 \uac01\uc778 \uae4a\uc774<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub0a0\uce74\ub85c\uc6b4 \ub0b4\ubd80 \ucf54\ub108 \ub610\ub294 \uae09\uaca9\ud55c \ub2e8\uba74 \ubcc0\ud654<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud558\uc911\uc120\uc774 \uc791\uc740 \ubc18\uacbd\uc73c\ub85c \ubab0\ub9ac\ubbc0\ub85c \uad6d\ubd80 \uc751\ub825\uc774 \ub178\uce58 \uacc4\uc218\ub9cc\ud07c \ud3c9\uade0\uc744 \ucd08\uacfc\ud569\ub2c8\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub3c4\uba74\uc758 \ud544\ub81b \ubc18\uacbd\uacfc \ubd80\ud488\uc5d0\uc11c \uce21\uc815\ud55c \ubc18\uacbd\uc758 \ube44\uad50<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ube44\uae08\uc18d \uac1c\uc7ac\ubb3c \ub610\ub294 \uc2a4\ud2b8\ub9c1\uac70<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\uc9c8 \uac1c\uc7ac\ubb3c\uc740 \uae30\uc9c0\uc640 \ube44\uc815\ud569\uc801\uc774\uc5b4\uc11c \uadf8 \ubcc0\ud615\uc744 \ub530\ub77c\uac08 \uc218 \uc5c6\uc2b5\ub2c8\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uac15\uc758 \uccad\uc815\ub3c4 \uc218\uc900, \uadf8\ub9ac\uace0 \ubd80\ud488\uc774 \ubd09\uc7ac\uc5d0\uc11c \uc704\uce58\ud55c \uacf3<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud0c8\ud0c4 \ub610\ub294 \uacfc\uce68\ud0c4\uce35<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud574\ub2f9 \uce35\uc740 \uacbd\ub3c4\uc640 \uc794\ub958 \uc751\ub825\uc5d0\uc11c \uc2ec\ubd80\uc640 \ub2e4\ub974\uba70, \uc790\uccb4\uc801\uc778 \uc751\ub825 \uc0c1\ud0dc\ub97c \uac00\uc9d1\ub2c8\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacbd\ud654 \uc804 \uc81c\uac70\ub41c \uc18c\uc7ac\ub7c9\uacfc \ub178 atmosphere\uc758 \ud0c4\uc18c \ud3ec\ud150\uc15c<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5b5\uc9c0 \ub07c\uc6cc\ub9de\ucda4 \ub610\ub294 \ud074\ub7a8\ud504 \uccb4\uacb0\ubd80<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub07c\uc6cc\ub9de\ucda4\uc740 \uc751\ub825 \uc9d1\uc911\uc774\uba70, \uccb4\uacb0\ubd80\uac00 \ubc8c\uc5b4\uc9c0\uba74 \uadf8 \uc704\uc5d0 \ud504\ub808\ud305 \uc190\uc0c1\uc774 \ucd94\uac00\ub429\ub2c8\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc811\ucd09 \uc555\ub825, \uadf8\ub9ac\uace0 \ubd80\ud488\uc774 \uc11c\ub85c \uc0c1\ub300\uc801\uc73c\ub85c \uc6c0\uc9c1\uc774\ub3c4\ub85d \uc124\uacc4\ub418\uc5c8\ub294\uc9c0 \uc5ec\ubd80<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubd80\uc2dd \ud53c\ud2b8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud53c\ud2b8\ub294 \ub178\uce58\uc774\uba70, \uade0\uc5f4\uc744 \uacc4\uc18d \uc9c4\ud589\uc2dc\ud0a4\ub294 \uc804\ud574\uc9c8\uc744 \ub2f4\uace0 \uc788\uc2b5\ub2c8\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud45c\uba74\uc774 \ubcf4\ud638\ub418\uc5c8\ub294\uc9c0 \uc5ec\ubd80, \uadf8\ub9ac\uace0 \ud30c\ub2e8\uba74\uc758 \uce68\uc804\ubb3c\uc5d0 \ud3ec\ud568\ub41c \uc131\ubd84<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc544\ud06c \uc190\uc0c1 \ub610\ub294 \uc6a9\uc811 \ubcf4\uc218<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uad6d\ubd80 \uc6a9\uc735\uacfc \uc7ac\uacbd\ud654\ub294 \uc794\ub958 \uc778\uc7a5 \uc0c1\ud0dc\uc758 \ucde8\uc131 \uc601\uc5ed\uc744 \ub0a8\uae41\ub2c8\ub2e4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uacf5\uad6c\uc758 \ubcf4\uc218 \uc774\ub825, \uadf8\ub9ac\uace0 \ubcf4\uc218 \ubd80\uc704\uc758 \uacbd\ub3c4<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\uacf5\uad6c\uc5d0\uc11c \ud53c\ub85c \uade0\uc5f4\uc774 \uc2dc\uc791\ub418\ub294 \uc704\uce58, \ud574\ub2f9 \ud615\uc0c1\uc774 \uc751\ub825\uc744 \uc9d1\uc911\uc2dc\ud0a4\ub294 \uc774\uc720, \uadf8\ub9ac\uace0 \uadf8 \ubd80\uc704\ub97c \uacf5\uc815 \ub2e8\uacc4\uc640 \uc5f0\uacb0\ud558\ub294 \uc810\uac80 \uc0ac\ud56d. \ucd9c\ucc98\uc758 \uace0\uc7a5 \uc2dd\ubcc4 \uc139\uc158\uc5d0\uc11c \ud3b8\uc9d1\ud568.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc2dc\uc810\uc5d0 \uad00\ud55c \ub450 \uac00\uc9c0 \uc0ac\uc2e4\uc774 \ub17c\uc758\uc758 \uac00\uce58\ub97c \uacb0\uc815\ud569\ub2c8\ub2e4. \ub2e8\uc21c \ud53c\ub85c\uc5d0\uc11c\ub294 \uade0\uc5f4 \uac1c\uc2dc\uac00 \uc804\uccb4 \uc218\uba85\uc758 \uc57d 90\ud37c\uc13c\ud2b8\ub97c \ucc28\uc9c0\ud560 \uc218 \uc788\uc73c\ubbc0\ub85c, \ubd80\ud488\uc740 \ubc1c\uacac\ud560 \uade0\uc5f4\uc774 \uc0dd\uae30\uae30 \uc804\uc5d0 \uc218\uba85\uc758 \uac70\uc758 \uc804\ubd80\ub97c \uc18c\ube44\ud558\uba70, \uc11c\ub958\uc0c1 \ub109\ub109\ud574 \ubcf4\uc774\ub294 \uac80\uc0ac \uc8fc\uae30\uac00 \uc218\uba85\uc758 \ub300\ubd80\ubd84\uc774 \ub420 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc811\ucd09\ubd80\uc5d0 \ud504\ub808\ud305\ub3c4 \uc874\uc7ac\ud558\uba74 \uac1c\uc2dc\ub294 \uc218\uba85\uc758 \uc57d 55\ud37c\uc13c\ud2b8\ub85c \ub5a8\uc5b4\uc9c0\uace0 \uac15\ub3c4 \uac10\uc18c \uacc4\uc218\ub294 2\uc5d0\uc11c 5 \uc774\uc0c1\uc73c\ub85c \uc0c1\uc2b9\ud558\ub294\ub370, \uc774\uac83\uc774 \uc6c0\uc9c1\uc774\ub3c4\ub85d \uc124\uacc4\ub418\uc9c0 \uc54a\uc740 \uccb4\uacb0\ubd80\uac00 \uacf5\uad6c\ub97c \uc870\uae30\uc5d0 \uc783\ub294 \ub9e4\uc6b0 \ud6a8\uacfc\uc801\uc778 \ubc29\ubc95\uc778 \uc774\uc720\uc785\ub2c8\ub2e4. \uadf8 \uc30d\uc758 \ud504\ub808\ud305 \uce21\uba74\uc740 \ub2e4\uc74c\uc5d0\uc11c \ub2e4\ub8f9\ub2c8\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/fretting-wear-tool-steel\/\">\uacf5\uad6c\uc758 \ud504\ub808\ud305 \ub9c8\ubaa8<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud53c\ub85c \ud30c\uad34\ub294 \uc124\uacc4 \uacb0\ud568\ub9cc\ud07c\uc774\ub098 \uccad\uc815\ub3c4 \uacb0\ud568\uc774\uba70, \uc7ac\uc6a9\ud574 \uacf5\uc815\uc774 \ubc14\ub85c \uc774 \ub54c\ubb38\uc5d0 \ub3c4\uc785\ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" src=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg\" alt=\"S-N curves for tension-compression fatigue testing of transverse A2 tool steel, air melted against electroslag remelted (ESR), stress against number of cycles\"\/><figcaption class=\"wp-element-caption\">\uadf8\ub9bc 11.1. \ud69f\ubc29\ud5a5 A2 \uacf5\uad6c\uac15 \uc2dc\ud3b8\uc758 \uc778\uc7a5-\uc555\ucd95 \ud53c\ub85c \uc2dc\ud5d8 S-N \uace1\uc120\uc73c\ub85c, \uacf5\uae30 \uc6a9\ud574\uc7ac\uc640 \uc804\uae30 \uc2ac\ub798\uadf8 \uc7ac\uc6a9\ud574(ESR)\uc7ac\ub97c \ube44\uad50\ud55c\ub2e4. ESR \uc2dc\ud3b8\uc740 \ud45c\uc2dc\ub41c \uc804 \uc218\uba85 \uad6c\uac04\uc5d0\uc11c \uacf5\uae30 \uc6a9\ud574\uc7ac\ubcf4\ub2e4 \uc704\uc5d0 \uc704\uce58\ud558\uba70, \ud654\uc0b4\ud45c\ub294 \ucc9c\ub9cc \uc0ac\uc774\ud074\uc744 \ud1b5\uacfc\ud558\uace0\ub3c4 \ud30c\ub2e8\ub418\uc9c0 \uc54a\uc740 \ub7f0\uc544\uc6c3 \uc2dc\ud5d8\uc744 \ub098\ud0c0\ub0b8\ub2e4. \ub450 \uace1\uc120\uc740 \uac19\uc740 \uac15\uc885\uc774\ubbc0\ub85c \uadf8 \ucc28\uc774\ub294 \uc7ac\uc6a9\ud574\uac00 \uc81c\uac70\ud558\ub294 \uac1c\uc7ac\ubb3c \ud568\ub7c9\uc774\ub2e4. \ucd9c\ucc98: E. Essadiqi, Tool Steels, in Steel Heat Treatment: Metallurgy and Technologies (G.E. Totten, ed.), CRC Press, 2006, Fig. 11.1.<\/figcaption><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">\uade0\uc5f4\uc744 \uc2dc\uc791\uc2dc\ud0a4\uc9c0 \uc54a\uace0 \ubd80\ud488\uc5d0 \ub9c8\ud0b9\ud558\uae30<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc2dd\ubcc4 \ub9c8\ud06c\ub294 \uacf5\uad6c\uac00 \uc644\uc131\ub41c \ud6c4\uc5d0 \uc801\uc6a9\ub418\uba70 \uc124\uacc4\uc758 \uc77c\ubd80\uac00 \uc544\ub2c8\uba70, \ubc14\ub85c \uadf8 \uc810\uc774 \ubb38\uc81c\ub97c \uc77c\uc73c\ud0b5\ub2c8\ub2e4. \ucd9c\ucc98\ub294 \uc120\ud638 \uc21c\uc11c\uc5d0 \ub300\ud574 \uc9c1\uc811\uc801\uc73c\ub85c \uc5b8\uae09\ud569\ub2c8\ub2e4. \uc591\uac01 \ubb38\uc790\ub294 \uc74c\uac01 \ubb38\uc790\ubcf4\ub2e4 \uc88b\uc740\ub370, \uc591\uac01 \ub9c8\ud06c\ub294 \uae08\uc18d\uc744 \ubcc0\uc704\uc2dc\ud0a4\ub294 \ub300\uc2e0 \uc7ac\ub8cc\ub97c \ucd94\uac00\ud558\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \ub9c8\ud06c\ub97c \uc74c\uac01\ud574\uc57c \ud558\ub294 \uacbd\uc6b0\uc5d0\ub294 \ub0c9\uac04 \uacf5\uc815\ubcf4\ub2e4 \uc5f4\uac04 \uacf5\uc815\uc774 \uc120\ud638\ub418\uba70, \ub9c8\ud0b9 \uc789\ud06c\uac00 \uc804\uae30 \uc5d0\uce6d \ud39c\uc774\ub098 \uc9c4\ub3d9 \uc870\uac01\uae30\ubcf4\ub2e4 \uc120\ud638\ub429\ub2c8\ub2e4. \uadf8 \uc138 \uac00\uc9c0 \uc74c\uac01 \ubc29\ubc95\uc740 \ubaa8\ub450 \ub0c9\uac04 \uac15 \uac01\uc778\ubcf4\ub2e4 \uc5ec\uc804\ud788 \ub35c \ud574\ub86d\uc2b5\ub2c8\ub2e4. \uac01\uc778\uc774 \ubd88\uac00\ud53c\ud55c \uacbd\uc6b0\uc5d0\ub294 \ubb38\uc790\uc758 \ub0a0\uce74\ub85c\uc6b4 \ubaa8\uc11c\ub9ac\ub97c \uc81c\uac70\ud55c \uc800\uc751\ub825 \uac01\uc778, \ub610\ub294 \ubb34\ub518 \uac01\uc778\uc774 \uc190\uc0c1\uc744 \uac00\uc7a5 \uc801\uac8c \uc8fc\uba70, \ud2b9\ud788 \uac01\uc778\uc774 \uc595\uc744 \ub54c \uadf8\ub7ec\ud558\uba70, \uac01\uc778\uc740 \ud544\ub81b\uc774\ub098 \ub2e8\uba74 \ubcc0\ud654 \uc606\uc774 \uc544\ub2c8\ub77c \uc54c\ub824\uc9c4 \uc800\uc751\ub825 \ubd80\uc704\uc5d0 \uc704\uce58\ud574\uc57c \ud569\ub2c8\ub2e4. \uae38\uace0 \uace7\uc740 \ud68d\uc744 \uac00\uc9c4 \ubb38\uc790\uac00 \uade0\uc5f4\uc744 \uc2dc\uc791\uc2dc\ud0ac \uacbd\ud5a5\uc774 \uac00\uc7a5 \ud07d\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ub9c8\ud0b9 \ubc29\ubc95<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud45c\uba74\uc5d0 \ubbf8\uce58\ub294 \uc601\ud5a5<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud5c8\uc6a9\ub418\ub294 \uc704\uce58<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc591\uac01 \ubb38\uc790, \uc8fc\uc870 \ub610\ub294 \ub2e8\uc870\ub85c \ud615\uc131<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc7ac\ub8cc\uac00 \uc81c\uac70\ub418\uc9c0 \uc54a\uace0 \ucd94\uac00\ub418\ubbc0\ub85c \ub178\uce58\uac00 \uc0dd\uae30\uc9c0 \uc54a\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud615\uc0c1\uc774 \uc591\uac01 \ub9c8\ud06c\ub97c \ud5c8\uc6a9\ud558\ub294 \ubaa8\ub4e0 \uc704\uce58<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub9c8\ud0b9 \uc789\ud06c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub9c8\ud06c\uac00 \ucf54\ud305\uc774\uba70 \ud45c\uba74\uc774 \uc190\uc0c1\ub418\uc9c0 \uc54a\uc74c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubaa8\ub4e0 \uae30\uacc4 \uac00\uacf5 \ud45c\uba74<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc804\uae30 \uc5d0\uce6d \ud39c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud45c\uba74 \uc190\uc0c1\uc774 \uc801\uc740 \uad6d\ubd80 \uac00\uc5f4<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc800\uc751\ub825 \uc601\uc5ed \ubc0f \ube44\uc784\uacc4 \ud45c\uba74<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc9c4\ub3d9 \uae30\uacc4 \uc870\uac01\uae30<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubc14\ub2e5\uc5d0 \ubbf8\uc138\ud55c \ub77c\uc6b4\ub4dc\uac00 \uc788\ub294 \uc5f0\uc18d \ud648<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc800\uc751\ub825 \uc601\uc5ed\uc5d0\ub9cc \uc801\uc6a9, \ud544\ub81b\uc744 \uac00\ub85c\uc9c8\ub7ec\uc11c\ub294 \uc548 \ub428<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc5f4\uac04 \uc2a4\ud0ec\ud551<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uae08\uc18d\uc774 \uace0\uc628\uc5d0\uc11c \uc5f0\uc131 \uc0c1\ud0dc\ub85c \ubcc0\ud615\ub418\uc5b4 \uc595\uc740 \ub178\uce58\ub97c \ub0a8\uae40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc800\uc751\ub825 \uc601\uc5ed, \ub0c9\uac04 \uc2a4\ud0ec\ud551\ubcf4\ub2e4 \uc120\ud638\ub428<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub0c9\uac04 \uac15\uc7ac \uc2a4\ud0ec\ud504<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uae08\uc18d\uc774 \ub0c9\uac04\uc5d0\uc11c \ubcc0\ud615\ub418\uc5b4 \ub0a0\uce74\ub85c\uc6b4 \ubc14\ub2e5 \ub178\uce58\uc640 \uc8fc\ubcc0\uc5d0 \uc794\ub958 \uc778\uc7a5 \uc751\ub825\uc744 \ub0a8\uae40<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc54c\ub824\uc9c4 \uc800\uc751\ub825 \uc601\uc5ed\uc5d0\ub9cc, \uac00\ubccd\uac8c \uc801\uc6a9<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ud070 \ub9c8\ud06c\uc758 \ub0c9\uac04 \ucf54\uc774\ub2dd<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub178\uce58 \uae4a\uc774\uc640 \uc794\ub958 \uc751\ub825 \ubaa8\ub450\uc5d0\uc11c \uac00\uc7a5 \uc2ec\uac01\ud55c \ubc29\ubc95<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ubc18\ubcf5 \ud558\uc911\uc744 \ubc1b\ub294 \ubaa8\ub4e0 \uacf5\uad6c\uc5d0\uc11c \ud68c\ud53c<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ucd9c\ucc98\uc5d0\uc11c \uc81c\uc2dc\ud55c \uc21c\uc11c\ub300\ub85c \uc2dd\ubcc4 \ub9c8\ud0b9 \ubc29\ubc95, \ud45c\uba74\uc5d0 \uac00\uc7a5 \ub35c \uc190\uc0c1\ub418\ub294 \uac83\ubd80\ud130 \uac00\uc7a5 \uc190\uc0c1\ub418\ub294 \uac83\uae4c\uc9c0. \ucd9c\ucc98: \uae30\uc0ac Fatigue Failures\uc758 \uc2dd\ubcc4 \ub9c8\ud0b9 \uaddc\uce59.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\ud658\uacbd\uc774 \uac1c\uc785\ud560 \ub54c<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ubd80\uc2dd \ud53c\ub85c\ub294 \ubc18\ubcf5 \uc751\ub825\uacfc \ud658\uacbd\uc758 \uc870\ud569\uc73c\ub85c, \uc5b4\ub290 \ud558\ub098\ub9cc\uc73c\ub85c\ub294 \ubd80\ud488\uc744 \uade0\uc5f4\uc2dc\ud0a4\uc9c0 \uc54a\uc2b5\ub2c8\ub2e4. \uadf8 \uc2e4\uc81c\uc801 \ud2b9\uc9d5\uc740 \uc8fc \uade0\uc5f4 \uc606\uc758 \uc791\uc740 \uade0\uc5f4 \uadf8\ub8f9, \ud45c\uba74\uc5d0 \uc555\ucc29\ub41c \ubd80\uc2dd \uc0dd\uc131\ubb3c, \uadf8\ub9ac\uace0 \ub9e4 \uc0ac\uc774\ud074\uc758 \uc555\ucd95 \ubc18\uc8fc\uae30\uac00 \ub450 \uba74\uc744 \ud568\uaed8 \ub20c\ub7ec \ub9c8\ubaa8\ub418\uace0 \ubcc0\uc0c9\ub41c \uae30\uc6d0\ubd80\uc785\ub2c8\ub2e4. \ud0c4\uc18c\uac15\uc5d0\uc11c \uade0\uc5f4\uc740 \uc885\uc885 \ubc18\uad6c\ud615 \ubd80\uc2dd \ud53c\ud2b8\uc5d0\uc11c \uc2dc\uc791\ub418\uc9c0\ub9cc, \ud53c\ud305\uc774 \ud544\uc218 \uc870\uac74\uc740 \uc544\ub2c8\uba70, \uacbd\ub85c\ub294 \uc77c\ubc18\uc801\uc73c\ub85c \uc785\uacc4\ub97c \ud1b5\uacfc\ud558\uba70 \uc57d\uac04\uc758 \ubd84\uc9c0\ub97c \ubcf4\uc785\ub2c8\ub2e4. \uade0\uc5f4\uc758 \uc218\ub294 \uc720\uc6a9\ud55c \ud310\ubcc4 \uae30\uc900\uc785\ub2c8\ub2e4. \uc5ec\ub7ec \ubd80\uc2dd \ud53c\ub85c \uade0\uc5f4\uc740 \uc885\uc885 \ud3c9\ud589 \uacbd\ub85c\ub97c \ub530\ub77c \ub098\ub780\ud788 \uc131\uc7a5\ud558\ub294 \ubc18\uba74, \uae30\uacc4\uc801 \ud53c\ub85c \uade0\uc5f4\uc740 \uac19\uc740 \uc601\uc5ed\uc758 \uc5ec\ub7ec \uc9c0\uc810\uc5d0\uc11c \uc2dc\uc791\ub420 \uc218 \uc788\uc9c0\ub9cc \uade0\uc5f4\uc774 \uba40\ub9ac \uc9c4\ud589\ub418\uae30 \uc804\uc5d0 \uadf8 \uc911 \ud558\ub098\uac00 \uc9c0\ubc30\uc801\uc774 \ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uac80\uc0ac \uc21c\uc11c\uac00 \uc911\uc694\ud558\uba70, \uc99d\uac70\ub97c \uc77d\uae30 \uc804\uc5d0 \ud30c\uad34\ud558\uae30 \uc27d\uc2b5\ub2c8\ub2e4. \ucd9c\ucc98\uc5d0\uc11c \uc81c\uc2dc\ud55c \uccab \ub2e8\uacc4\ub294 \uc140\ub8f0\ub85c\uc624\uc2a4 \uc544\uc138\ud14c\uc774\ud2b8 \ud14c\uc774\ud504\ub098 \ud50c\ub77c\uc2a4\ud2f1 \ubcf5\uc81c \uc7ac\ub8cc\ub85c \ud30c\ub2e8\uba74\uc744 \uc2a4\ud2b8\ub9bd\ud558\uc5ec \ub098\uc911 \ubd84\uc11d\uc744 \uc704\ud574 \uce68\uc804\ubb3c\uc744 \ud3ec\uc9d1\ud558\ub294 \uac83\uc785\ub2c8\ub2e4. \uadf8\ub7f0 \ub2e4\uc74c \ubd80\ud488\uc744 \ucd08\uc74c\ud30c \ud0f1\ud06c\uc5d0\uc11c \uc2dc\uc57d \ub4f1\uae09 \uc544\uc138\ud1a4\uc73c\ub85c \uc138\ucc99 \ubc0f \ud0c8\uc9c0\ud558\ub294\ub370, \uc544\uc138\ud1a4\uc740 \uc140\ub8f0\ub85c\uc624\uc2a4 \uc544\uc138\ud14c\uc774\ud2b8 \uc794\ub958\ubb3c\uc744 \uc81c\uac70\ud558\uace0 \uc790\ubd84 \ud0d0\uc0c1 \ud604\ud0c1\uc561\uacfc \ub300\ubd80\ubd84\uc758 \uc561\uccb4 \uce68\ud22c\uc81c\ub97c \uc6a9\ud574\ud558\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \ube0c\ub7ec\uc2dc\ub85c \uc6a9\ub9e4\ub97c \uc801\uc6a9\ud558\ub294 \uac83\uc740 \uad6c\uccb4\uc801\uc73c\ub85c \uc774 \ubc29\ubc95\uc774 \uc544\ub2d9\ub2c8\ub2e4. \uae30\uc6d0\ubd80\uc758 \ubd80\uc2dd \uc0dd\uc131\ubb3c\uc740 \uc800\ubc30\uc728\uc5d0\uc11c \uc624\ub3c4\ud560 \uc218 \uc788\uc73c\uba70, \uad6c\ud615 \ub610\ub294 \uacb0\uc808\ud615 \uc0b0\ud654\ubb3c\uc774 \uc785\uacc4 \ud30c\uba74\uc73c\ub85c \uc27d\uac8c \uc624\uc778\ub420 \uc218 \uc788\uc73c\ubbc0\ub85c \uc678\uad00\ub9cc\uc73c\ub85c \uacb0\ub860\uc744 \ub0b4\ub824\uc11c\ub294 \uc548 \ub429\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ud569\uaca9 \uacb0\uc815\uc5d0 \ubc18\uc601\ud560 \uc218\uce58\ub294 \ud53c\ub85c \ud55c\uacc4\uc778\ub370, \uc774\ub294 \ud658\uacbd\uc5d0\uc11c \uc0b4\uc544\ub0a8\uc9c0 \ubabb\ud558\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. \uc5f0\uac15\uc758 \ud53c\ub85c \ud55c\uacc4\ub294 \uc804\uae30\ud654\ud559\uc801 \uc804\uc704\uc5d0 \ub530\ub77c \uc218\uc131 \uc870\uac74\uc5d0\uc11c \uc81c\uac70\ub418\uba70, \ud30c\uad34\ub97c \uc77c\uc73c\ud0a4\ub294 \ub370 \ud544\uc694\ud55c \uc751\ub825 \ubc94\uc704\ub294 \uc2dc\uac04\uacfc \uc0ac\uc774\ud074 \uc218\uac00 \uc99d\uac00\ud568\uc5d0 \ub530\ub77c \uc810\uc9c4\uc801\uc73c\ub85c \uac10\uc18c\ud569\ub2c8\ub2e4. \uc774\uac83\uc774 \ubd80\uc2dd \ud53c\ub85c \uc2dc\ud5d8\uc774 \ucd1d \uc218\uba85\uc774 \uc544\ub2cc \ud658\uacbd\uc5d0\uc11c\uc758 \uade0\uc5f4 \uc131\uc7a5 \uc18d\ub3c4\ub97c \uce21\uc815\ud558\ub294 \uc774\uc720\uc774\uba70, \uc2b5\uc724 \ub610\ub294 \uc218\uc18c \ud568\uc720 \uc11c\ube44\uc2a4\uc5d0\uc11c \ubc18\ubcf5\ub418\ub294 \ubd80\ud488\uc774 \uacf5\uae30 \uc911\uc5d0\uc11c \uce21\uc815\ub41c \ud55c\uacc4\uc5d0 \ub300\ud574 \ucd9c\ud558\ub420 \uc218 \uc5c6\ub294 \uc774\uc720\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uacf5\uad6c\uac00 \uad6c\ub974\uac70\ub098 \ubbf8\ub044\ub7ec\uc9c0\ub294 \uc811\ucd09 \ud53c\ub85c<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\uc811\ucd09 \ud53c\ub85c\ub294 \ubc18\ubcf5 \uad6c\ub984 \ub610\ub294 \uad6c\ub984\uacfc \ubbf8\ub044\ub7fc\uc774 \uacb0\ud569\ub41c \ub450 \uace1\uba74\uc758 \ud30c\uad34\uc774\uba70, \uc911\uc694\ud55c \uc751\ub825\uc740 \ubd80\ud488\uc774 \uc6c0\uc9c1\uc77c \ub54c \ubc29\ud5a5\uc774 \ubc18\uc804\ub418\ub294 \uad50\ubc88 \uc804\ub2e8 \uc751\ub825\uc785\ub2c8\ub2e4. \uc21c\uc218 \uad6c\ub984\uc5d0\uc11c \uadf8 \uc804\ub2e8 \uc751\ub825\uc740 \ud45c\uba74 \uc57d\uac04 \uc544\ub798\uc5d0\uc11c \ucd5c\ub300\uac00 \ub418\ubbc0\ub85c \uc678\ubd80\uc5d0\uc11c \uac74\uc804\ud574 \ubcf4\uc774\ub294 \uc7ac\ub8cc\uc5d0\uc11c \uade0\uc5f4\uc774 \uc2dc\uc791\ub420 \uc218 \uc788\uace0, \ub098\uc911\uc5d0 \ud53c\ud2b8\ub85c \ud45c\uba74\uc5d0 \ub3c4\ub2ec\ud569\ub2c8\ub2e4. \ubbf8\ub044\ub7fc\uc774 \ucd94\uac00\ub418\uba74 \ub9c8\ucc30\uc774 \ucd5c\ub300 \uc804\ub2e8 \uc751\ub825\uc744 \ud45c\uba74\uc5d0 \ub354 \uac00\uae5d\uac8c \uc774\ub3d9\uc2dc\ud0a4\uace0 \uadf8 \ud06c\uae30\ub97c \uc99d\uac00\uc2dc\ud0a4\ubbc0\ub85c, \uae30\uc5b4 \uc774\ub294 \uc811\ucd09\uc774 \uc21c\uc218 \uad6c\ub984\uc778 \ud53c\uce58 \ub77c\uc778 \uc704\uac00 \uc544\ub2c8\ub77c \ud53c\uce58 \ub77c\uc778 \uc606\uc5d0\uc11c \ud53c\ud305\ub429\ub2c8\ub2e4. \ub9c8\uc774\ud06c\ub85c\ud53c\ud305\uc740 \ub2e4\uc2dc \ub354 \ubbf8\uc138\ud55c \uaddc\ubaa8\ub85c \uc7ac\ub8cc\ub97c \uc81c\uac70\ud558\uba70, \ud558\uc911\uc5d0 \ube44\ud574 \ub108\ubb34 \uc587\uc740 \ucf00\uc774\uc2a4\ub294 \ucf00\uc774\uc2a4\uc640 \ucf54\uc5b4 \uc0ac\uc774\uc758 \uacc4\uba74\uc5d0\uc11c \ud30c\uad34\ub418\ub294\ub370, \ucd9c\ucc98\ub294 \uc774 \ubaa8\ub4dc\ub97c \uc11c\ube0c\ucf00\uc774\uc2a4 \ud53c\ub85c \ub610\ub294 \ucf00\uc774\uc2a4 \ud06c\ub7ec\uc2f1\uc774\ub77c\uace0 \ubd80\ub985\ub2c8\ub2e4.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uc774 \uc8fc\uc81c\uc758 \uc6a9\uc5b4\ub294 \uc624\ub7ab\ub3d9\uc548 \ubb38\uc81c\uc600\ub294\ub370, \ubca0\uc5b4\ub9c1\uacfc \uae30\uc5b4 \uc0b0\uc5c5\uc774 \ub3d9\uc77c\ud55c \uc190\uc0c1\uc744 \ub2e4\ub978 \uc774\ub984\uc73c\ub85c \ubd88\ub800\uae30 \ub54c\ubb38\uc785\ub2c8\ub2e4. ANSI\/AGMA 1010-E96\uc774 \uc774\ub97c \ud574\uacb0\ud558\uae30 \uc704\ud574 \ubc1c\ud589\ub418\uc5c8\uc73c\uba70, \ubcf4\uace0\uc11c\uc5d0\uc11c \uac00\uc7a5 \uc911\uc694\ud55c \ub450 \uac00\uc9c0 \ubcc0\uacbd\uc740 \uc2a4\ud3f4\ub9c1 \ub300\uc2e0 \ub9e4\ud06c\ub85c\ud53c\ud305\uc744, \ud544\ub9c1 \ub300\uc2e0 \ub9c8\uc774\ud06c\ub85c\ud53c\ud305\uc744 \uc0ac\uc6a9\ud574\uc57c \ud55c\ub2e4\ub294 \uac83\uc785\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\uc2a4\ucf00\uc77c<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ud45c\uc900\uc774 \uc720\uc9c0\ud558\ub294 \uc6a9\uc5b4<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uc0ad\uc81c\ud560 \uc6a9\uc5b4<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uac70\uc2dc\uc801 \uaddc\ubaa8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub9e4\ud06c\ub85c\ud53c\ud305, \ud53c\ud305, \ucd08\uae30 \ud53c\ud305, \ud30c\uad34\uc801 \ud53c\ud305, \ud50c\ub808\uc774\ud0b9, \ud53c\ub85c \ub9c8\ubaa8, \uc11c\ube0c\ucf00\uc774\uc2a4 \ud53c\ub85c \ub610\ub294 \ucf00\uc774\uc2a4 \ud06c\ub7ec\uc2f1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc2a4\ud3f4\ub9c1, \uc5ec\ub7ec \ub2e4\ub978 \uba54\ucee4\ub2c8\uc998\uc5d0 \uc801\uc6a9\ub418\uc5b4 \ubaa8\ud638\ud568<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ubbf8\uc2dc\uc801 \uaddc\ubaa8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub9c8\uc774\ud06c\ub85c\ud53c\ud305, \ub9c8\uc774\ud06c\ub85c\uc2a4\ud3f4\ub9c1, \ud504\ub85c\uc2a4\ud305, \uae00\ub808\uc774\uc9d5, \uadf8\ub808\uc774 \uc2a4\ud14c\uc774\ub2dd, \ud45c\uba74 \uc190\uc0c1<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud544\ub9c1, \ub9c8\uc774\ud06c\ub85c\ud53c\ud305\uc758 \uc678\uad00\uc774\ub098 \uba54\ucee4\ub2c8\uc998\uc744 \uc124\uba85\ud558\uc9c0 \ubabb\ud568<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>ANSI\/AGMA 1010-E96\uc5d0 \uc758\ud574 \uc815\ub82c\ub41c \uc811\ucd09 \ud53c\ub85c \uc6a9\uc5b4, \ubca0\uc5b4\ub9c1\uacfc \uae30\uc5b4 \uc0b0\uc5c5\uc774 \ub3d9\uc77c\ud55c \uc190\uc0c1\uc744 \ub3d9\uc77c\ud55c \ubc29\uc2dd\uc73c\ub85c \uc124\uba85\ud558\ub3c4\ub85d \ubc1c\ud589\ub428. \ucd9c\ucc98: \uae30\uc0ac Fatigue Failures\uc758 \ud45c 1.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\uacf5\uad6c\uac15 \uc8fc\ubb38\uc5d0\uc11c \uadf8 \ud45c\uc900\uc758 \uc720\uc6a9\ud55c \ubd80\ubd84\uc740 \ubaa8\ub4dc\uc640 \uc774\ub97c \uc81c\uc5b4\ud558\ub294 \uc694\uc778 \uc0ac\uc774\uc758 \uc5f0\uacb0\uc785\ub2c8\ub2e4. \uc544\ub798 \ud45c\uc758 \ub2e4\uc12f \uac00\uc9c0 \ubaa8\ub4dc \uc911 \uc138 \uac00\uc9c0\ub294 \uc724\ud65c\uc758 \uc601\ud5a5\uc744 \ubc1b\uc73c\uba70, \ud45c\uba74\uc5d0\uc11c \uc2dc\uc791\ud558\ub294 \ubaa8\ub4e0 \ubaa8\ub4dc\ub97c \ud3ec\ud568\ud558\uace0, \ud45c\uba74 \uc544\ub798\uc5d0\uc11c \uc2dc\uc791\ud558\ub294 \ub450 \uac00\uc9c0\ub294 \ub300\uc2e0 \uc7ac\ub8cc\uc5d0 \uc758\ud574 \uacb0\uc815\ub429\ub2c8\ub2e4. \uac1c\uc7ac\ubb3c \uae30\uc6d0 \uc811\ucd09 \ud53c\ub85c\ub294 \ubbf8\ub044\ub7fc \ubca0\uc5b4\ub9c1\uc758 \uc8fc\uc694 \ubaa8\ub4dc\uc774\uba70, \uc774\ub294 \uacbd\ud654 \uc0b0\ud654\ubb3c \uac1c\uc7ac\ubb3c\uacfc \uadf8\ub4e4\uc774 \ud615\uc131\ud558\ub294 \uc2a4\ud2b8\ub9c1\uac70\uc758 \ud06c\uae30\uc640 \ubc00\ub3c4\uc5d0 \uc758\ud574 \uc81c\uc5b4\ub418\ubbc0\ub85c \uc9c4\uacf5 \ucc98\ub9ac \uac15\uc774 \uc0ac\uc6a9\ub418\ub294 \uc774\uc720\uc785\ub2c8\ub2e4. \uc11c\ube0c\ucf00\uc774\uc2a4 \ud53c\ub85c\ub294 \uac15 \uccad\uc815\ub3c4 \ubb38\uc81c\uac00 \uc544\ub2cc \uc124\uacc4 \ubc0f \uc5f4\ucc98\ub9ac \ubb38\uc81c\uc774\uba70, \ud574\uacb0\ucc45\uc740 \ucf00\uc774\uc2a4 \uae4a\uc774\ub97c \ub298\ub9ac\uac70\ub098 \ucf54\uc5b4 \uacbd\ub3c4\ub97c \ub192\uc774\ub294 \uac83\uc774\uba70, \uc774\uac00 \uc644\uc804 \uacbd\ud654\ub418\uc5b4 \ucde8\uc131\uc774 \ub418\uc9c0 \uc54a\ub3c4\ub85d \uc8fc\uc758 \uae4a\uac8c \uc801\uc6a9\ud574\uc57c \ud569\ub2c8\ub2e4.<\/p>\n\n\n\n<figure class=\"wp-block-table is-style-stripes\"><table class=\"has-fixed-layout\"><thead><tr><th class=\"has-text-align-left\" data-align=\"left\">\ubaa8\ub4dc<\/th><th class=\"has-text-align-left\" data-align=\"left\">\uae30\uc6d0\uc774 \uc704\uce58\ud558\ub294 \uacf3<\/th><th class=\"has-text-align-left\" data-align=\"left\">\ubc1c\uc0dd \uc5ec\ubd80\ub97c \uc81c\uc5b4\ud558\ub294 \uc694\uc778<\/th><\/tr><\/thead><tbody><tr><td class=\"has-text-align-left\" data-align=\"left\">\uac1c\uc7ac\ubb3c \uae30\uc6d0, \ud45c\uba74 \uc544\ub798<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc811\ucd09\ubd80 \uc544\ub798, \ucd5c\ub300 \uad50\ubc88 \uc804\ub2e8 \uc751\ub825 \uae4a\uc774 \uc704\uc758 \ube44\uae08\uc18d \uac1c\uc7ac\ubb3c\uc5d0\uc11c<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc0b0\ud654\ubb3c \ubc0f \uae30\ud0c0 \uacbd\uc9c8 \uac1c\uc7ac\ubb3c\uc758 \ud06c\uae30\uc640 \ubc00\ub3c4, \uadf8\ub9ac\uace0 \ub2e4\ub978 \ubaa8\ub4dc\uc758 \ubd80\uc7ac<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc11c\ube0c\ucf00\uc774\uc2a4 \ud53c\ub85c, \ucf00\uc774\uc2a4 \ud06c\ub7ec\uc2f1\uc774\ub77c\uace0\ub3c4 \ud568<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ucf00\uc774\uc2a4\uc640 \ucf54\uc5b4 \uc0ac\uc774\uc758 \uacbd\uacc4 \uadfc\ucc98<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uace1\ub960 \ubc18\uacbd\uacfc \ud558\uc911\uc5d0 \ube44\ud574 \ub108\ubb34 \uc587\uc740 \ucf00\uc774\uc2a4, \ub610\ub294 \uc811\ucd09 \uc751\ub825\uc5d0 \ube44\ud574 \ub108\ubb34 \ub0ae\uc740 \ucf54\uc5b4 \uacbd\ub3c4<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uc810 \ud45c\uba74 \uae30\uc6d0<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc811\ucd09 \ud45c\uba74\uc5d0\uc11c, \uc724\ud65c\uc720 \ub9c9\uc774 \ub3cc\uae30\ub97c \ubd84\ub9ac\ud558\uc9c0 \ubabb\ud558\ub294 \uacf3<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0ae\uc740 \uc724\ud65c\uc720 \uc810\ub3c4, \uc811\ucd09 \ub3cc\uae30\ubcf4\ub2e4 \uc587\uc740 \ub9c9, \uc811\uc120 \ubc29\ud5a5 \ud798\uacfc \uc2ec\ud55c \ubbf8\ub044\ub7fc<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\uae30\ud558\ud559\uc801 \uc751\ub825 \uc9d1\uc911<\/td><td class=\"has-text-align-left\" data-align=\"left\">\uc120 \uc811\ucd09\uc758 \ub05d\uc5d0\uc11c, \uc811\ucd09 \uc751\ub825\uc774 \uac00\uc7a5 \ub192\uc740 \uacf3<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub05d \uc811\ucd09 \ud615\uc0c1, \uc815\ub82c \ubd88\ub7c9, \uadf8\ub9ac\uace0 \uc801\uc6a9 \ud558\uc911 \ud558\uc758 \ucc98\uc9d0<\/td><\/tr><tr><td class=\"has-text-align-left\" data-align=\"left\">\ub9c8\uc774\ud06c\ub85c \ud53c\ud305<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ud45c\uba74\uc5d0\uc11c, \ub9e4\ud06c\ub85c \ud53c\ud305 \uc774\ud558\uc758 \uaddc\ubaa8<\/td><td class=\"has-text-align-left\" data-align=\"left\">\ub0ae\uc740 \uc810\ub3c4, \uc587\uc740 \ub9c9, \ud0c4\uc131 \uc720\uccb4\uc5ed\ud559\uc801 \uc555\ub825\uc758 \uc0c1\uc2e4, \uadf8\ub9ac\uace0 \ub290\ub9b0 \uc6b4\uc804 \uc18d\ub3c4<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>\ub2e4\uc12f \uac00\uc9c0 \uc811\ucd09 \ud53c\ub85c \ubaa8\ub4dc\uc640 \ucd9c\ucc98\uc5d0\uc11c \uac01\uac01\uc744 \uc81c\uc5b4\ud55c\ub2e4\uace0 \ub098\uc5f4\ud55c \uc694\uc778\ub4e4. \ub2e4\uc12f \uc911 \uc138 \uac00\uc9c0\ub294 \uc724\ud65c\uc758 \uc601\ud5a5\uc744 \ubc1b\uc73c\uba70, \uae30\uc6d0\uc774 \ud45c\uba74\uc5d0 \uc788\ub294 \ubaa8\ub4e0 \ubaa8\ub4dc\ub97c \ud3ec\ud568\ud55c\ub2e4. \ucd9c\ucc98: Fatigue Failures \uae30\uc0ac\uc758 Table 2.<\/em><\/p>\n\n\n\n<h2 class=\"wp-block-heading\">\uacf5\uad6c\uac15 \uc8fc\ubb38\uc5d0\uc11c \uc774\uac83\uc774 \uc758\ubbf8\ud558\ub294 \ubc14<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\ud53c\ub85c\ub294 \ub3c4\uba74, \uac15\uc7ac, \ud604\uc7a5 \uc791\uc5c5 \uad00\ud589\uc774 \ubaa8\ub450 \uc0ac\ud6c4\uc5d0 \ud310\ub3c5\ud560 \uc218 \uc788\ub294 \ud754\uc801\uc744 \ub0a8\uae30\ub294 \uc720\uc77c\ud55c \ud30c\uc190 \ubaa8\ub4dc\uc774\uba70, \ub3d9\uc77c\ud55c \ub3c4\uba74\uc73c\ub85c \ub610 \ub2e4\ub978 \uae08\ud615\uc744 \ub9cc\ub4e4\uae30 \uc804\uc5d0 \uadf8 \ud310\ub3c5\uc744 \uc218\ud589\ud560 \uac00\uce58\uac00 \uc788\ub2e4. \ub124 \uac00\uc9c0 \ud56d\ubaa9\uc774 \uae30\ub85d\uc5d0 \ud3ec\ud568\ub418\uc5b4\uc57c \ud55c\ub2e4. \uc2e4\uc81c\ub85c \uc0dd\uc131\ub41c \ud45c\uba74 \uc870\ub3c4\uc640 \ud544\ub81b \ubc18\uacbd, \uc65c\ub0d0\ud558\uba74 \ub178\uce58 \uacc4\uc218\ub294 \uc758\ub3c4\uac00 \uc544\ub2c8\ub77c \ud615\uc0c1\uc5d0 \uc758\ud574 \uacb0\uc815\ub418\uae30 \ub54c\ubb38\uc774\ub2e4. \ubaa8\ub4e0 \uc2dd\ubcc4 \ub9c8\ud06c\uc758 \uc704\uce58\uc640 \ubc29\ubc95, \uc65c\ub0d0\ud558\uba74 \uc751\ub825\uc774 \uc791\uc6a9\ud558\ub294 \uc601\uc5ed\uc758 \ub9c8\ud06c\ub294 \uc124\uacc4\ub41c \uade0\uc5f4 \uac1c\uc2dc\uc810\uc774\uae30 \ub54c\ubb38\uc774\ub2e4. \uac15\uc7ac\uc758 \uccad\uc815\ub3c4 \uc218\uc900, \uac1c\uc7ac\ubb3c\uc774 \ubb38\uc81c\uac00 \ub420 \ub9cc\ud07c \uc811\ucd09 \uc751\ub825\uc774 \ub192\uc740 \uacbd\uc6b0. \uadf8\ub9ac\uace0 \ud45c\uba74 \ucc98\ub9ac, \uc65c\ub0d0\ud558\uba74 \ud45c\uba74\uc758 \uc555\ucd95\uce35\uc740 \uac1c\uc2dc \uc218\uba85\uc744 \ud655\ubcf4\ud558\uba70 \ud615\uc0c1\uc744 \ubcc0\uacbd\ud560 \uc218 \uc5c6\ub294 \uacbd\uc6b0\uc758 \ud45c\uc900 \ud574\ub2f5\uc774\uae30 \ub54c\ubb38\uc774\ub2e4. \uadf8 \uce35\uc774 \ubcc0\ud654\uc2dc\ud0a4\ub294 \uc794\ub958 \uc751\ub825\uc740 \ub2e4\uc74c\uacfc \uac19\uc774 \ubcf4\uace0\ub41c\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/residual-stress-measurement-tooling\/\">\uacf5\uad6c\uc758 \uc794\ub958 \uc751\ub825 \uce21\uc815<\/a> \uc5d0\uc11c \uc124\uba85\ud558\ub294 \ubc29\uc2dd\uc73c\ub85c, \uadf8\ub9ac\uace0 \ud45c\uba74\uc774 \uc2dc\uc791\ud558\ub294 \uc0c1\ud0dc\ub97c \uacb0\uc815\ud558\ub294 \uc5f4\ucc98\ub9ac \ub2e8\uacc4\ub294 \ub2e4\uc74c\uc5d0 \uc81c\uc2dc\ub418\uc5b4 \uc788\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/quench-cracking-tool-steel\/\">\uacf5\uad6c\uac15\uc758 \ub2f4\uae08\uc9c8 \uade0\uc5f4<\/a>. \ud30c\ub2e8\uba74 \uc790\uccb4\uc758 \ud754\uc801 \ub4a4\uc5d0 \uc788\ub294 \uba54\ucee4\ub2c8\uc998\uc740 \ub2e4\uc74c\uc5d0 \uc81c\uc2dc\ub418\uc5b4 \uc788\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/fracture-surface-features-chart\/\">\ud30c\ub2e8\uba74 \ud2b9\uc9d5 \ubc0f \uadf8 \uc758\ubbf8<\/a>, \uacf5\uad6c \ub610\ub294 \uae08\ud615 \ud30c\uc190\uc758 \ub2e8\uacc4\ubcc4 \uc6d0\uc778\uc740 \ub2e4\uc74c\uc5d0 \uc788\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/tool-and-die-failure-analysis\/\">\uacf5\uad6c \ubc0f \uae08\ud615 \uace0\uc7a5 \ubd84\uc11d<\/a>, \uadf8\ub9ac\uace0 \ud30c\ub2e8\uc774 \uc124\uba85\ub418\uae30 \uc804\uc5d0 \ubd84\ub958\ub418\ub294 \ubc29\uc2dd\uc740 \ub2e4\uc74c\uc5d0 \uc788\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/damage-mode-identification-chart\/\">\uc190\uc0c1 \ubaa8\ub4dc \uc2dd\ubcc4 \ucc28\ud2b8<\/a>. \ucda9\uaca9 \ubc0f \ubc18\ubcf5 \uc0ac\uc6a9\uc744 \uc704\ud55c \uc778\uc131 \ub4f1\uae09\uc740 \ub2e4\uc74c \uc544\ub798\uc5d0 \ubd84\ub958\ub418\uc5b4 \uc788\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steels-for-cracking-resistance\/\">\uade0\uc5f4 \uc800\ud56d\uc131\uc744 \uc704\ud55c \uacf5\uad6c\uac15<\/a>, \ub4f1\uae09\uc774 \ud761\uc218\ud558\ub294 \ucda9\uaca9 \uc5d0\ub108\uc9c0\ub294 \ub2e4\uc74c\uc5d0 \uae30\ub85d\ub418\uc5b4 \uc788\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/charpy-impact-test-tool-steel\/\">\uacf5\uad6c\uac15\uc758 \uc0e4\ub974\ud53c \ucda9\uaca9 \uc2dc\ud5d8<\/a>, \uadf8\ub9ac\uace0 \ud30c\uad34 \uc778\uc131 \ub370\uc774\ud130\ub294 \ub2e4\uc74c\uc5d0 \uc788\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-fracture-toughness-chart\/\">\uacf5\uad6c\uac15 \ud30c\uad34 \uc778\uc131 \ucc28\ud2b8<\/a>, \uadf8\ub9ac\uace0 \uadf8 \uc218\uce58 \ub4a4\uc758 \uc870\uc9c1\uc744 \uac80\uc0ac\ud558\ub294 \ubc29\uc2dd\uc740 \ub2e4\uc74c\uc5d0 \uc81c\uc2dc\ub418\uc5b4 \uc788\ub2e4 <a href=\"https:\/\/aobosteel.com\/ko\/tool-steel-microstructure\/\">\uacf5\uad6c\uac15 \ubbf8\uc138\uc870\uc9c1<\/a>.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">\ud53c\ub85c \uc9c4\ub2e8\uc5d0 \ub530\ub77c \uc870\uce58\ud558\uae30 \uc804\uc5d0<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">\ucc38\uace0 \ud398\uc774\uc9c0\uc774\uba70, Aobo Steel\uc758 \uc0ac\uc591\uc774 \uc544\ub2c8\uace0, \uc704\uc758 \uc218\uce58\ub294 \uba85\uc2dc\ub41c \ud2b9\uc815 \uc2dc\ub8cc\uc640 \ud569\uae08\uc5d0 \ub300\ud574 \ubc1c\ud45c\ub41c \uac12\uc774\ub2e4. \ud53c\ub85c \uc218\uba85\uc740 \uc2e4\uc81c \uc751\ub825 \uc774\ub825, \ud615\uc0c1, \ud45c\uba74 \uc0c1\ud0dc \ubc0f \ud658\uacbd\uc5d0 \ub530\ub77c \ub2ec\ub77c\uc9c0\uba70, \uc774 \uc911 \uc5b4\ub290 \uac83\ub3c4 \ub2e8\uc77c \ud30c\ub2e8 \uc0ac\uc9c4\uc5d0\uc11c \ubcf5\uc6d0\ud560 \uc218 \uc5c6\ub2e4. \ud30c\ub2e8\uba74\uc758 \ub9e4\ub044\ub7ec\uc6b4 \uc601\uc5ed\uc740 \uc810\uc9c4\uc801 \uc131\uc7a5\uc758 \uc99d\uac70\uc774\uc9c0 \uadf8 \uc790\uccb4\ub85c \uc5b4\ub5a4 \ud558\uc911\uc774 \uadf8\uac83\uc744 \uc0dd\uc131\ud588\ub294\uc9c0\uc5d0 \ub300\ud55c \uc99d\uba85\uc774 \uc544\ub2c8\uba70, \uae30\uc6d0\ubd80\uc758 \ubd80\uc2dd \uc0dd\uc131\ubb3c\uc740 \uc800\ubc30\uc728\uc5d0\uc11c \ud30c\ub2e8 \ud2b9\uc9d5\uc73c\ub85c \uc624\uc778\ub420 \uc218 \uc788\ub2e4. \uc138\ucc99 \uc804\uc5d0 \ud45c\uba74\uc744 \uc2a4\ud2b8\ub9bd\ud558\uace0 \uae30\ub85d\ud558\uba70, \ubaa8\ub4e0 \uc218\uba85 \uc218\uce58\ub294 \uadf8\uac83\uc774 \ub098\uc628 \uac80\uc0ac \uc8fc\uae30\uc5d0 \uc5f0\uacc4\ub41c \ucd94\uc815\uce58\ub85c \ucde8\uae09\ud558\ub77c.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\ucd9c\ucc98: ASM Handbook, Volume 11, Failure Analysis and Prevention, ASM International, 2002.<\/p>","protected":false},"excerpt":{"rendered":"<p>Fatigue Failure in Tool Steel A tool that fails in fatigue passed the checks the drawing asked for. The hardness is on specification, the grade is the one the application called for, and the load never exceeded the design value. The crack still started, usually at a feature nobody specified, and it grew a little [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"parent":0,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"_uag_custom_page_level_css":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"normal-width-container","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"disabled","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"class_list":["post-21170","page","type-page","status-publish","hentry"],"yoast_head":"<!-- This site is optimized with the Yoast SEO Premium plugin v28.9 (Yoast SEO v28.9) - https:\/\/yoast.com\/product\/yoast-seo-premium-wordpress\/ -->\n<title>Fatigue Failure in Tool Steel: Where the Crack Starts | Aobo Steel<\/title>\n<meta name=\"description\" content=\"Where a fatigue crack starts on a hardened tool, how marking and finishing practice decides it, how corrosion fatigue is identified, and the contact fatigue modes with the factors that control each one. Reference data from ASM Handbook Volume 11.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/aobosteel.com\/ko\/tool-steel-fatigue-failure\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Fatigue Failure in Tool Steel\" \/>\n<meta property=\"og:description\" content=\"Where a fatigue crack starts on a hardened tool, how marking and finishing practice decides it, how corrosion fatigue is identified, and the contact fatigue modes with the factors that control each one. Reference data from ASM Handbook Volume 11.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/aobosteel.com\/ko\/tool-steel-fatigue-failure\/\" \/>\n<meta property=\"og:site_name\" content=\"AoboSteel\" \/>\n<meta property=\"article:publisher\" content=\"https:\/\/www.facebook.com\/profile.php?id=61565368220197\" \/>\n<meta property=\"article:modified_time\" content=\"2026-10-15T17:40:54+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data1\" content=\"13\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"TechArticle\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/\"},\"author\":{\"name\":\"Evan\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\"},\"headline\":\"Fatigue Failure in Tool Steel\",\"datePublished\":\"2026-10-07T12:19:01+00:00\",\"dateModified\":\"2026-10-15T17:40:54+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/\"},\"wordCount\":2641,\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg\",\"inLanguage\":\"ko-KR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/\",\"name\":\"Fatigue Failure in Tool Steel: Where the Crack Starts | Aobo Steel\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg\",\"datePublished\":\"2026-10-07T12:19:01+00:00\",\"dateModified\":\"2026-10-15T17:40:54+00:00\",\"description\":\"Where a fatigue crack starts on a hardened tool, how marking and finishing practice decides it, how corrosion fatigue is identified, and the contact fatigue modes with the factors that control each one. Reference data from ASM Handbook Volume 11.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/#primaryimage\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2026\\\/10\\\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/tool-steel-fatigue-failure\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"\u9996\u9875\",\"item\":\"https:\\\/\\\/aobosteel.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Fatigue Failure in Tool Steel\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#website\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"name\":\"AoboSteel\",\"description\":\"\",\"publisher\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/aobosteel.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#organization\",\"name\":\"AoboSteel\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"contentUrl\":\"https:\\\/\\\/aobosteel.com\\\/wp-content\\\/uploads\\\/2025\\\/01\\\/cropped-aobo-steel-1.avif\",\"width\":1052,\"height\":592,\"caption\":\"AoboSteel\"},\"image\":{\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\"]},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/aobosteel.com\\\/#\\\/schema\\\/person\\\/96118415c30ca6bb52eaf1127b052ef7\",\"name\":\"Evan\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g\",\"caption\":\"Evan\"},\"sameAs\":[\"http:\\\/\\\/www.aobosteel.com\",\"https:\\\/\\\/www.facebook.com\\\/profile.php?id=61565368220197\",\"https:\\\/\\\/www.instagram.com\\\/aobosteel\\\/\",\"https:\\\/\\\/www.linkedin.com\\\/in\\\/aobosteel-evan\\\/\",\"https:\\\/\\\/x.com\\\/AobosteelEvan\",\"https:\\\/\\\/www.youtube.com\\\/@aobosteel\"],\"url\":\"https:\\\/\\\/aobosteel.com\\\/ko\\\/blog\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO Premium plugin. -->","yoast_head_json":{"title":"\uacf5\uad6c\uac15 \ud53c\ub85c \ud30c\uad34: \uade0\uc5f4 \uc2dc\uc791 \uc704\uce58 | Aobo Steel","description":"\uacbd\ud654\ub41c \uacf5\uad6c\uc5d0\uc11c \ud53c\ub85c \uade0\uc5f4\uc774 \uc2dc\uc791\ub418\ub294 \uc704\uce58, \ub9c8\ud0b9\uacfc \ub9c8\ubb34\ub9ac \uacf5\uc815\uc774 \uc774\ub97c \uacb0\uc815\ud558\ub294 \ubc29\uc2dd, \ubd80\uc2dd \ud53c\ub85c\uc758 \uc2dd\ubcc4 \ubc29\ubc95, \uadf8\ub9ac\uace0 \uac01 \ubaa8\ub4dc\ub97c \uc9c0\ubc30\ud558\ub294 \uc778\uc790\uc640 \ud568\uaed8 \uc811\ucd09 \ud53c\ub85c \ubaa8\ub4dc\ub97c \ub2e4\ub8f9\ub2c8\ub2e4. ASM Handbook Volume 11 \ucc38\uc870 \ub370\uc774\ud130.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/aobosteel.com\/ko\/tool-steel-fatigue-failure\/","og_locale":"ko_KR","og_type":"article","og_title":"Fatigue Failure in Tool Steel","og_description":"Where a fatigue crack starts on a hardened tool, how marking and finishing practice decides it, how corrosion fatigue is identified, and the contact fatigue modes with the factors that control each one. Reference data from ASM Handbook Volume 11.","og_url":"https:\/\/aobosteel.com\/ko\/tool-steel-fatigue-failure\/","og_site_name":"AoboSteel","article_publisher":"https:\/\/www.facebook.com\/profile.php?id=61565368220197","article_modified_time":"2026-10-15T17:40:54+00:00","og_image":[{"url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg","type":"","width":"","height":""}],"twitter_card":"summary_large_image","twitter_misc":{"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"13\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"TechArticle","@id":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/#article","isPartOf":{"@id":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/"},"author":{"name":"Evan","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7"},"headline":"Fatigue Failure in Tool Steel","datePublished":"2026-10-07T12:19:01+00:00","dateModified":"2026-10-15T17:40:54+00:00","mainEntityOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/"},"wordCount":2641,"publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg","inLanguage":"ko-KR"},{"@type":"WebPage","@id":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/","url":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/","name":"\uacf5\uad6c\uac15 \ud53c\ub85c \ud30c\uad34: \uade0\uc5f4 \uc2dc\uc791 \uc704\uce58 | Aobo Steel","isPartOf":{"@id":"https:\/\/aobosteel.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/#primaryimage"},"image":{"@id":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/#primaryimage"},"thumbnailUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg","datePublished":"2026-10-07T12:19:01+00:00","dateModified":"2026-10-15T17:40:54+00:00","description":"\uacbd\ud654\ub41c \uacf5\uad6c\uc5d0\uc11c \ud53c\ub85c \uade0\uc5f4\uc774 \uc2dc\uc791\ub418\ub294 \uc704\uce58, \ub9c8\ud0b9\uacfc \ub9c8\ubb34\ub9ac \uacf5\uc815\uc774 \uc774\ub97c \uacb0\uc815\ud558\ub294 \ubc29\uc2dd, \ubd80\uc2dd \ud53c\ub85c\uc758 \uc2dd\ubcc4 \ubc29\ubc95, \uadf8\ub9ac\uace0 \uac01 \ubaa8\ub4dc\ub97c \uc9c0\ubc30\ud558\ub294 \uc778\uc790\uc640 \ud568\uaed8 \uc811\ucd09 \ud53c\ub85c \ubaa8\ub4dc\ub97c \ub2e4\ub8f9\ub2c8\ub2e4. ASM Handbook Volume 11 \ucc38\uc870 \ub370\uc774\ud130.","breadcrumb":{"@id":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/"]}]},{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/#primaryimage","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2026\/10\/Aobo-Steel-Tool-Steel-Fatigue-totten-fig-11-1-sn-curves-air-melted-esr-a2.jpg"},{"@type":"BreadcrumbList","@id":"https:\/\/aobosteel.com\/tool-steel-fatigue-failure\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"\u9996\u9875","item":"https:\/\/aobosteel.com\/"},{"@type":"ListItem","position":2,"name":"Fatigue Failure in Tool Steel"}]},{"@type":"WebSite","@id":"https:\/\/aobosteel.com\/#website","url":"https:\/\/aobosteel.com\/","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","description":"","publisher":{"@id":"https:\/\/aobosteel.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/aobosteel.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/aobosteel.com\/#organization","name":"\uc544\uc624\ubcf4\uc2a4\ud2f8","url":"https:\/\/aobosteel.com\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/","url":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","contentUrl":"https:\/\/aobosteel.com\/wp-content\/uploads\/2025\/01\/cropped-aobo-steel-1.avif","width":1052,"height":592,"caption":"AoboSteel"},"image":{"@id":"https:\/\/aobosteel.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/"]},{"@type":"Person","@id":"https:\/\/aobosteel.com\/#\/schema\/person\/96118415c30ca6bb52eaf1127b052ef7","name":"\uc5d0\ubc18","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/8e402f2e6f36093f0bf1855dbf79269cde23cd659c44eefdd7ecf7ff9c05786f?s=96&d=mm&r=g","caption":"Evan"},"sameAs":["http:\/\/www.aobosteel.com","https:\/\/www.facebook.com\/profile.php?id=61565368220197","https:\/\/www.instagram.com\/aobosteel\/","https:\/\/www.linkedin.com\/in\/aobosteel-evan\/","https:\/\/x.com\/AobosteelEvan","https:\/\/www.youtube.com\/@aobosteel"],"url":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"}]}},"uagb_featured_image_src":{"full":false,"thumbnail":false,"medium":false,"medium_large":false,"large":false,"1536x1536":false,"2048x2048":false,"trp-custom-language-flag":false},"uagb_author_info":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"uagb_comment_info":0,"uagb_excerpt":"Fatigue Failure in Tool Steel A tool that fails in fatigue passed the checks the drawing asked for. The hardness is on specification, the grade is the one the application called for, and the load never exceeded the design value. The crack still started, usually at a feature nobody specified, and it grew a little&hellip;","rttpg_featured_image_url":null,"rttpg_author":{"display_name":"Evan","author_link":"https:\/\/aobosteel.com\/ko\/blog\/author\/admin\/"},"rttpg_comment":0,"rttpg_category":null,"rttpg_excerpt":"Fatigue Failure in Tool Steel A tool that fails in fatigue passed the checks the drawing asked for. The hardness is on specification, the grade is the one the application called for, and the load never exceeded the design value. The crack still started, usually at a feature nobody specified, and it grew a little&hellip;","_links":{"self":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21170","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/comments?post=21170"}],"version-history":[{"count":3,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21170\/revisions"}],"predecessor-version":[{"id":22674,"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/pages\/21170\/revisions\/22674"}],"wp:attachment":[{"href":"https:\/\/aobosteel.com\/ko\/wp-json\/wp\/v2\/media?parent=21170"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}